<rss version="2.0"><channel><title>&#x41A;&#x43E;&#x43D;&#x43A;&#x443;&#x440;&#x441; &#xAB;&#x421;&#x434;&#x435;&#x43B;&#x430;&#x43D;&#x43E; &#x441;&#x432;&#x43E;&#x438;&#x43C;&#x438; &#x440;&#x443;&#x43A;&#x430;&#x43C;&#x438;&#xBB; Latest Topics</title><link>https://websvarka.ru/talk/forum/46-konkurs-%C2%ABsdelano-svoimi-rukami%C2%BB/</link><description>&#x41A;&#x43E;&#x43D;&#x43A;&#x443;&#x440;&#x441; &#xAB;&#x421;&#x434;&#x435;&#x43B;&#x430;&#x43D;&#x43E; &#x441;&#x432;&#x43E;&#x438;&#x43C;&#x438; &#x440;&#x443;&#x43A;&#x430;&#x43C;&#x438;&#xBB; Latest Topics</description><language>en</language><item><title>&#x420;&#x435;&#x437;&#x443;&#x43B;&#x44C;&#x442;&#x430;&#x442;&#x44B; &#x41A;&#x43E;&#x43D;&#x43A;&#x443;&#x440;&#x441;&#x430; &#xAB;&#x421;&#x434;&#x435;&#x43B;&#x430;&#x43D;&#x43E; &#x441;&#x432;&#x43E;&#x438;&#x43C;&#x438; &#x440;&#x443;&#x43A;&#x430;&#x43C;&#x438;&#xBB;</title><link>https://websvarka.ru/talk/topic/4005-rezultaty-konkursa-%C2%ABsdelano-svoimi-rukami%C2%BB/</link><description><![CDATA[<p>Конкурс завершен и самое время подвести его итоги. Конкурс «Сделано своими руками» — это не просто первый конкурс на форуме Вебсварка, но это и первый конкурс сварщиков, организованный в интернете в таких масштабах. Чуть позже у нас будет возможность обсудить все его плюсы и минусы (создам отдельную тему), а пока давайте порадуемся за победителей, скажем спасибо всем участникам и спонсорам.<br /><br />Таблица результатов конкурса в порядке убывания голосов<br /></p><div class="ipsSpoiler" data-ipsspoiler=""><div class="ipsSpoiler_header"><span></span></div><div class="ipsSpoiler_contents"><p><span>http://websvarka.ru/images/forum/itogi-1.jpg</span></p></div></div><p><br /><span style="font-size:18px;">Победители Конкурса «Сделано своими руками»</span></p><ul><li><strong>1-е место</strong> занимает <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/3288-mirotvorets/" data-ipshover-target="http://87.239.109.236/talk/profile/3288-mirotvorets/?do=hovercard" data-mentionid="3288" rel="">@Миротворец</a></strong> с Конкурсной работой №46 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3851" rel="external nofollow">Мои помощники, облегчающие работу</a> </strong>и получает в качестве приза<strong> <strong>Сварочный инвертор</strong> РЕСАНТА САИ 250ПРОФ</strong></li><li><strong>2-е место</strong> занимает <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/612-sergeykl/" data-ipshover-target="http://87.239.109.236/talk/profile/612-sergeykl/?do=hovercard" data-mentionid="612" rel="">@СергейКл</a></strong> с Конкурсной работой №22 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3749" rel="external nofollow">Компактная печь на отработанном масле</a></strong> и получает в качестве приза<strong> <strong>Сварочный инвертор</strong> СВАРОГ ARC 205 (J96)</strong></li><li><strong>3-е место</strong> занимает <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/10079-reankor-2002/" data-ipshover-target="http://87.239.109.236/talk/profile/10079-reankor-2002/?do=hovercard" data-mentionid="10079" rel="">@Reankor 2002</a></strong> с Конкурсной работой №14 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3725" rel="external nofollow">Динозавр</a></strong> и получает в качестве приза<strong> Сварочный инвертор Aurora MINIONE 1600 с аксессуарами в кейсе</strong></li></ul><p><strong>Поздравляем!</strong><br /><br /><span style="font-size:18px;">Поощрительные призы</span><br /><strong>11 поощрительных призов в размере 1000 руб.</strong> достаются Участникам, занявшим с 4 по 14 места в результате общего голосования (более 30 голосов или &gt;2% в итоговой таблице). Это:</p><ul><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/7618-yuriy-ivanov/" data-ipshover-target="http://87.239.109.236/talk/profile/7618-yuriy-ivanov/?do=hovercard" data-mentionid="7618" rel="">@Юрий Иванов</a></strong> с Конкурсной работой №36 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3815" rel="external nofollow">Мангал «Олень»</a></strong></li><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/9346-bokor/" data-ipshover-target="http://87.239.109.236/talk/profile/9346-bokor/?do=hovercard" data-mentionid="9346" rel="">@Bokor</a></strong> с Конкурсной работой №53 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3882" rel="external nofollow">Восставшие из титана</a></strong></li><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11199-outlaw/" data-ipshover-target="http://87.239.109.236/talk/profile/11199-outlaw/?do=hovercard" data-mentionid="11199" rel="">@Outlaw</a></strong> с Конкурсной работой №23 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3750" rel="external nofollow">Чоппер</a></strong></li><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/699-belazz/" data-ipshover-target="http://87.239.109.236/talk/profile/699-belazz/?do=hovercard" data-mentionid="699" rel="">@BelaZZ</a></strong> с Конкурсной работой №3 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3652" rel="external nofollow">Коптилка</a></strong></li><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11068-darthwelder/" data-ipshover-target="http://87.239.109.236/talk/profile/11068-darthwelder/?do=hovercard" data-mentionid="11068" rel="">@DarthWelder</a></strong> с Конкурсной работой №5 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3656" rel="external nofollow">Автомобильный навес и инструмент для его производства</a></strong></li><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11238-anton31/" data-ipshover-target="http://87.239.109.236/talk/profile/11238-anton31/?do=hovercard" data-mentionid="11238" rel="">@Anton31</a></strong> с Конкурсной работой №30 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3791" rel="external nofollow">Прицепы для внедорожников</a></strong></li><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11084-demitr/" data-ipshover-target="http://87.239.109.236/talk/profile/11084-demitr/?do=hovercard" data-mentionid="11084" rel="">@Demitr</a></strong> с Конкурсной работой №4 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3654" rel="external nofollow">Карета лимузин</a></strong></li><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/8109-mag/" data-ipshover-target="http://87.239.109.236/talk/profile/8109-mag/?do=hovercard" data-mentionid="8109" rel="">@MAG</a></strong> с Конкурсной работой №18 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3734" rel="external nofollow">Драконы</a></strong></li><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/9906-varkapodarka/" data-ipshover-target="http://87.239.109.236/talk/profile/9906-varkapodarka/?do=hovercard" data-mentionid="9906" rel="">@varkapodarka</a></strong> с Конкурсной работой №19 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3740" rel="external nofollow">Набор рюмок «На сома»</a></strong></li><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11140-nub/" data-ipshover-target="http://87.239.109.236/talk/profile/11140-nub/?do=hovercard" data-mentionid="11140" rel="">@Nub</a></strong> с Конкурсной работой №16 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3727" rel="external nofollow">Братья Стали</a></strong></li><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11360-vera/" data-ipshover-target="http://87.239.109.236/talk/profile/11360-vera/?do=hovercard" data-mentionid="11360" rel="">@vera</a></strong> с Конкурсной работой №65 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3919" rel="external nofollow">Муха Цокотуха</a></strong></li></ul><p><strong>Поздравляем!</strong><br /><br />Также, <strong>5 призов в размере 1000 руб.</strong> достаются Участникам, которых хотелось бы просто поощрить, независимо от количества полученных голосов. Это мой личный выбор, как Организатора. В этот список попали Работы: начинающих сварщиков; сделанные специально под Конкурс (или в его процессе); которые просто хочется поддержать. Это:</p><ul><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/10997-stepanyuk_vlad/" data-ipshover-target="http://87.239.109.236/talk/profile/10997-stepanyuk_vlad/?do=hovercard" data-mentionid="10997" rel="">@Степанюк_Влад</a></strong> с Конкурсной работой №1 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3643" rel="external nofollow">Павлинчик</a></strong></li><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/177-mitka51/" data-ipshover-target="http://87.239.109.236/talk/profile/177-mitka51/?do=hovercard" data-mentionid="177" rel="">@митька51</a></strong> с Конкурсной работой №41 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3841" rel="external nofollow">Бетономешалка</a></strong></li><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/9258-saper24/" data-ipshover-target="http://87.239.109.236/talk/profile/9258-saper24/?do=hovercard" data-mentionid="9258" rel="">@saper24</a></strong> с Конкурсной работой №51 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3872" rel="external nofollow">Шлем средневекового рыцаря</a></strong></li><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/4300-johnhess/" data-ipshover-target="http://87.239.109.236/talk/profile/4300-johnhess/?do=hovercard" data-mentionid="4300" rel="">@johnhess</a></strong> с Конкурсной работой №52 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3877" rel="external nofollow">Учение с увлечением</a></strong></li><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/10654-maks-kachalkin/" data-ipshover-target="http://87.239.109.236/talk/profile/10654-maks-kachalkin/?do=hovercard" data-mentionid="10654" rel="">@Макс Качалкин</a></strong> с Конкурсной работой №55 <strong><a href="http://websvarka.ru/talk/index.php?showtopic=3891" rel="external nofollow">Рыцарь заката</a></strong></li></ul><p><strong>Поздравляем!</strong><br /><br /><span style="font-size:18px;">Благодарность всем Участникам</span><br />Именно благодаря Вам Конкурс состоялся. Не расстраивайтесь, если в этом Конкурсе ничего не выиграли — побед без поражений не бывает.</p><ul><li><strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/10997-stepanyuk_vlad/" data-ipshover-target="http://87.239.109.236/talk/profile/10997-stepanyuk_vlad/?do=hovercard" data-mentionid="10997" rel="">@Степанюк_Влад</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11090-dimasik30/" data-ipshover-target="http://87.239.109.236/talk/profile/11090-dimasik30/?do=hovercard" data-mentionid="11090" rel="">@Dimasik30</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/699-belazz/" data-ipshover-target="http://87.239.109.236/talk/profile/699-belazz/?do=hovercard" data-mentionid="699" rel="">@BelaZZ</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11084-demitr/" data-ipshover-target="http://87.239.109.236/talk/profile/11084-demitr/?do=hovercard" data-mentionid="11084" rel="">@Demitr</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11068-darthwelder/" data-ipshover-target="http://87.239.109.236/talk/profile/11068-darthwelder/?do=hovercard" data-mentionid="11068" rel="">@DarthWelder</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/2095-zmey71/" data-ipshover-target="http://87.239.109.236/talk/profile/2095-zmey71/?do=hovercard" data-mentionid="2095" rel="">@zmey71</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11072-shtirlitz/" data-ipshover-target="http://87.239.109.236/talk/profile/11072-shtirlitz/?do=hovercard" data-mentionid="11072" rel="">@shtirlitz</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11099-vlad25/" data-ipshover-target="http://87.239.109.236/talk/profile/11099-vlad25/?do=hovercard" data-mentionid="11099" rel="">@влад25</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11078-chereev/" data-ipshover-target="http://87.239.109.236/talk/profile/11078-chereev/?do=hovercard" data-mentionid="11078" rel="">@Chereev</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11154-alekseipetrov/" data-ipshover-target="http://87.239.109.236/talk/profile/11154-alekseipetrov/?do=hovercard" data-mentionid="11154" rel="">@alekseipetrov</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/10307-krech/" data-ipshover-target="http://87.239.109.236/talk/profile/10307-krech/?do=hovercard" data-mentionid="10307" rel="">@krech</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11000-nikolay-pervyy/" data-ipshover-target="http://87.239.109.236/talk/profile/11000-nikolay-pervyy/?do=hovercard" data-mentionid="11000" rel="">@Николай первый</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11169-potap/" data-ipshover-target="http://87.239.109.236/talk/profile/11169-potap/?do=hovercard" data-mentionid="11169" rel="">@Потап</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/10079-reankor-2002/" data-ipshover-target="http://87.239.109.236/talk/profile/10079-reankor-2002/?do=hovercard" data-mentionid="10079" rel="">@Reankor 2002</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11168-_seryy_/" data-ipshover-target="http://87.239.109.236/talk/profile/11168-_seryy_/?do=hovercard" data-mentionid="11168" rel="">@_серый_</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11140-nub/" data-ipshover-target="http://87.239.109.236/talk/profile/11140-nub/?do=hovercard" data-mentionid="11140" rel="">@Nub</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/7603-svarchic/" data-ipshover-target="http://87.239.109.236/talk/profile/7603-svarchic/?do=hovercard" data-mentionid="7603" rel="">@svarchic</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/8109-mag/" data-ipshover-target="http://87.239.109.236/talk/profile/8109-mag/?do=hovercard" data-mentionid="8109" rel="">@MAG</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/9906-varkapodarka/" data-ipshover-target="http://87.239.109.236/talk/profile/9906-varkapodarka/?do=hovercard" data-mentionid="9906" rel="">@varkapodarka</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/5242-vvt1954/" data-ipshover-target="http://87.239.109.236/talk/profile/5242-vvt1954/?do=hovercard" data-mentionid="5242" rel="">@vvt1954</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/10998-jonny976/" data-ipshover-target="http://87.239.109.236/talk/profile/10998-jonny976/?do=hovercard" data-mentionid="10998" rel="">@Jonny976</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/612-sergeykl/" data-ipshover-target="http://87.239.109.236/talk/profile/612-sergeykl/?do=hovercard" data-mentionid="612" rel="">@СергейКл</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11199-outlaw/" data-ipshover-target="http://87.239.109.236/talk/profile/11199-outlaw/?do=hovercard" data-mentionid="11199" rel="">@Outlaw</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11210-ilyaognev/" data-ipshover-target="http://87.239.109.236/talk/profile/11210-ilyaognev/?do=hovercard" data-mentionid="11210" rel="">@ilyaognev</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11226-nikolay-svarschik/" data-ipshover-target="http://87.239.109.236/talk/profile/11226-nikolay-svarschik/?do=hovercard" data-mentionid="11226" rel="">@Николай Сварщик</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/10442-uriy/" data-ipshover-target="http://87.239.109.236/talk/profile/10442-uriy/?do=hovercard" data-mentionid="10442" rel="">@Урий</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/10154-solyan/" data-ipshover-target="http://87.239.109.236/talk/profile/10154-solyan/?do=hovercard" data-mentionid="10154" rel="">@solyan</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11233-izi/" data-ipshover-target="http://87.239.109.236/talk/profile/11233-izi/?do=hovercard" data-mentionid="11233" rel="">@Izi</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11244-egorushka/" data-ipshover-target="http://87.239.109.236/talk/profile/11244-egorushka/?do=hovercard" data-mentionid="11244" rel="">@Egorushka</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11238-anton31/" data-ipshover-target="http://87.239.109.236/talk/profile/11238-anton31/?do=hovercard" data-mentionid="11238" rel="">@Anton31</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/10751-alekc1964/" data-ipshover-target="http://87.239.109.236/talk/profile/10751-alekc1964/?do=hovercard" data-mentionid="10751" rel="">@alekc1964</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/1391-vnuk/" data-ipshover-target="http://87.239.109.236/talk/profile/1391-vnuk/?do=hovercard" data-mentionid="1391" rel="">@vnuk</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/9592-mutnyy/" data-ipshover-target="http://87.239.109.236/talk/profile/9592-mutnyy/?do=hovercard" data-mentionid="9592" rel="">@мутный</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/7971-sosnovskiy1/" data-ipshover-target="http://87.239.109.236/talk/profile/7971-sosnovskiy1/?do=hovercard" data-mentionid="7971" rel="">@sosnovskiy1</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/3573-svarik/" data-ipshover-target="http://87.239.109.236/talk/profile/3573-svarik/?do=hovercard" data-mentionid="3573" rel="">@Сварик</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/7618-yuriy-ivanov/" data-ipshover-target="http://87.239.109.236/talk/profile/7618-yuriy-ivanov/?do=hovercard" data-mentionid="7618" rel="">@Юрий Иванов</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/9160-kurt1/" data-ipshover-target="http://87.239.109.236/talk/profile/9160-kurt1/?do=hovercard" data-mentionid="9160" rel="">@Kurt1</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/7435-cimon/" data-ipshover-target="http://87.239.109.236/talk/profile/7435-cimon/?do=hovercard" data-mentionid="7435" rel="">@cimon</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/231-minotawr/" data-ipshover-target="http://87.239.109.236/talk/profile/231-minotawr/?do=hovercard" data-mentionid="231" rel="">@Minotawr</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/10497-koltsov67/" data-ipshover-target="http://87.239.109.236/talk/profile/10497-koltsov67/?do=hovercard" data-mentionid="10497" rel="">@koltsov67</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/177-mitka51/" data-ipshover-target="http://87.239.109.236/talk/profile/177-mitka51/?do=hovercard" data-mentionid="177" rel="">@митька51</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/5372-susanin/" data-ipshover-target="http://87.239.109.236/talk/profile/5372-susanin/?do=hovercard" data-mentionid="5372" rel="">@Сусанин</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11187-kuzmin/" data-ipshover-target="http://87.239.109.236/talk/profile/11187-kuzmin/?do=hovercard" data-mentionid="11187" rel="">@Kuzmin</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/10593-oyawrik/" data-ipshover-target="http://87.239.109.236/talk/profile/10593-oyawrik/?do=hovercard" data-mentionid="10593" rel="">@Oyawrik</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/5931-alrami/" data-ipshover-target="http://87.239.109.236/talk/profile/5931-alrami/?do=hovercard" data-mentionid="5931" rel="">@alrami</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/3288-mirotvorets/" data-ipshover-target="http://87.239.109.236/talk/profile/3288-mirotvorets/?do=hovercard" data-mentionid="3288" rel="">@Миротворец</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/9938-moglo/" data-ipshover-target="http://87.239.109.236/talk/profile/9938-moglo/?do=hovercard" data-mentionid="9938" rel="">@moglo</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11321-kreker33/" data-ipshover-target="http://87.239.109.236/talk/profile/11321-kreker33/?do=hovercard" data-mentionid="11321" rel="">@Kreker33</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/1894-morgmail/" data-ipshover-target="http://87.239.109.236/talk/profile/1894-morgmail/?do=hovercard" data-mentionid="1894" rel="">@morgmail</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11235-russia811/" data-ipshover-target="http://87.239.109.236/talk/profile/11235-russia811/?do=hovercard" data-mentionid="11235" rel="">@russia811</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/9258-saper24/" data-ipshover-target="http://87.239.109.236/talk/profile/9258-saper24/?do=hovercard" data-mentionid="9258" rel="">@saper24</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/4300-johnhess/" data-ipshover-target="http://87.239.109.236/talk/profile/4300-johnhess/?do=hovercard" data-mentionid="4300" rel="">@johnhess</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/9346-bokor/" data-ipshover-target="http://87.239.109.236/talk/profile/9346-bokor/?do=hovercard" data-mentionid="9346" rel="">@Bokor</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11333-dmitriy-sh/" data-ipshover-target="http://87.239.109.236/talk/profile/11333-dmitriy-sh/?do=hovercard" data-mentionid="11333" rel="">@Дмитрий Ш</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/10654-maks-kachalkin/" data-ipshover-target="http://87.239.109.236/talk/profile/10654-maks-kachalkin/?do=hovercard" data-mentionid="10654" rel="">@Макс Качалкин</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11340-sibirskysvarscik/" data-ipshover-target="http://87.239.109.236/talk/profile/11340-sibirskysvarscik/?do=hovercard" data-mentionid="11340" rel="">@SibirskySvarscik</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11342-alumboats/" data-ipshover-target="http://87.239.109.236/talk/profile/11342-alumboats/?do=hovercard" data-mentionid="11342" rel="">@alumboats</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/1842-valeron/" data-ipshover-target="http://87.239.109.236/talk/profile/1842-valeron/?do=hovercard" data-mentionid="1842" rel="">@Валерон</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/7662-sed_alex/" data-ipshover-target="http://87.239.109.236/talk/profile/7662-sed_alex/?do=hovercard" data-mentionid="7662" rel="">@sed_alex</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/3573-svarik/" data-ipshover-target="http://87.239.109.236/talk/profile/3573-svarik/?do=hovercard" data-mentionid="3573" rel="">@Сварик</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11352-surzhikov/" data-ipshover-target="http://87.239.109.236/talk/profile/11352-surzhikov/?do=hovercard" data-mentionid="11352" rel="">@Surzhikov</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/7520-gleb/" data-ipshover-target="http://87.239.109.236/talk/profile/7520-gleb/?do=hovercard" data-mentionid="7520" rel="">@Глеб</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/9285-kruazik/" data-ipshover-target="http://87.239.109.236/talk/profile/9285-kruazik/?do=hovercard" data-mentionid="9285" rel="">@круазик</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11356-kasyanov-eduard/" data-ipshover-target="http://87.239.109.236/talk/profile/11356-kasyanov-eduard/?do=hovercard" data-mentionid="11356" rel="">@Касьянов Эдуард</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11360-vera/" data-ipshover-target="http://87.239.109.236/talk/profile/11360-vera/?do=hovercard" data-mentionid="11360" rel="">@vera</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/7858-aleksey79/" data-ipshover-target="http://87.239.109.236/talk/profile/7858-aleksey79/?do=hovercard" data-mentionid="7858" rel="">@алексей79</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/2956-unforgiven48/" data-ipshover-target="http://87.239.109.236/talk/profile/2956-unforgiven48/?do=hovercard" data-mentionid="2956" rel="">@unforgiven48</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11361-89066586544/" data-ipshover-target="http://87.239.109.236/talk/profile/11361-89066586544/?do=hovercard" data-mentionid="11361" rel="">@89066586544</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11371-bibun/" data-ipshover-target="http://87.239.109.236/talk/profile/11371-bibun/?do=hovercard" data-mentionid="11371" rel="">@bibun</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11374-semensemenov/" data-ipshover-target="http://87.239.109.236/talk/profile/11374-semensemenov/?do=hovercard" data-mentionid="11374" rel="">@SemenSemenov</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11344-ernestu/" data-ipshover-target="http://87.239.109.236/talk/profile/11344-ernestu/?do=hovercard" data-mentionid="11344" rel="">@ernestu</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/4573-avia/" data-ipshover-target="http://87.239.109.236/talk/profile/4573-avia/?do=hovercard" data-mentionid="4573" rel="">@Avia</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11364-nikolay/" data-ipshover-target="http://87.239.109.236/talk/profile/11364-nikolay/?do=hovercard" data-mentionid="11364" rel="">@Nikолай</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/11409-bays/" data-ipshover-target="http://87.239.109.236/talk/profile/11409-bays/?do=hovercard" data-mentionid="11409" rel="">@Bays</a></strong>, <strong><a contenteditable="false" data-ipshover="" href="https://websvarka.ru/talk/profile/9066-amateur/" data-ipshover-target="http://87.239.109.236/talk/profile/9066-amateur/?do=hovercard" data-mentionid="9066" rel="">@Amateur</a></strong></li></ul><p><strong>Спасибо!</strong><br /><br /><span style="font-size:18px;">Благодарность Спонсорам</span><br />Отдельные слова благодарности выражаю Спонсорам — они поддержали идею Конкурса тогда, когда не было никакой информации ни о возможном количестве участников, ни вообще о возможном интересе к такого рода конкурсам в интернете. Для тех, кто забыл — это:</p><ul><li><strong><a href="http://resanta.ru/" rel="external nofollow">Ресанта</a></strong> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</li><li><strong><a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a></strong> — первый интернет-гипермаркет сварочного оборудования.</li><li><strong><a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a></strong> — интернет-магазин строительного оборудования.</li></ul><p><span style="font-size:18px;">Получение призов</span><br />В ближайшие дни я свяжусь с каждым победителем для обсуждения всех деталей.<br /><br />Объявляю Конкурс закрытым!</p>]]></description><guid isPermaLink="false">4005</guid><pubDate>Tue, 04 Mar 2014 09:55:19 +0000</pubDate></item><item><title>&#x41C;&#x43E;&#x438; &#x43F;&#x43E;&#x43C;&#x43E;&#x449;&#x43D;&#x438;&#x43A;&#x438;, &#x43E;&#x431;&#x43B;&#x435;&#x433;&#x447;&#x430;&#x44E;&#x449;&#x438;&#x435; &#x440;&#x430;&#x431;&#x43E;&#x442;&#x443;</title><link>https://websvarka.ru/talk/topic/3851-moi-pomoschniki-oblegchayuschie-rabotu/</link><description><![CDATA[
<p>Всем привет! Хочу поделится своими прибамбасами которые изготовил сам: вальцовочный станок, стойка для радиаторов, подъемник, трактор. Всех этих помощником сделал для облегчения своего труда.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1-0-07540100-1392114175.jpg" data-fileid="29816" data-fileext="jpg" rel=""><img data-fileid="29816" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-07540100-1392114175_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1-0-07540100-1392114175_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1-0-80765100-1392114180.jpg" data-fileid="29818" data-fileext="jpg" rel=""><img data-fileid="29818" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-80765100-1392114180_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1-0-80765100-1392114180_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1-0-17619300-1392114179.jpg" data-fileid="29817" data-fileext="jpg" rel=""><img data-fileid="29817" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-17619300-1392114179_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1-0-17619300-1392114179_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1-0-99615900-1392114182.jpg" data-fileid="29819" data-fileext="jpg" rel=""><img data-fileid="29819" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-99615900-1392114182_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1-0-99615900-1392114182_thumb.jpg"></a></p><p> </p><p> </p><p>
<strong>Вальцовочный станок 3 в одном: листогиб, трубогиб и зиговка</strong></p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1-0-55702100-1392114887.jpg" data-fileid="29821" data-fileext="jpg" rel=""><img data-fileid="29821" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-55702100-1392114887_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1-0-55702100-1392114887_thumb.jpg"></a></p><p> </p><p>
Станок имеет электропривод на вращение двух нижних валов, электропривод подъёма нижнего бокового вала и откидной механизм верхнего вала. Рабочая длина валов составляет 1600 мм и вальцует ст3 до 2 мм до диаметра 160 мм. Зиговка тоже работает до 2 мм. Трубогиб для круглой и квадратной трубы до 40. Оба имеют сменные ролики под разные форматы. В общей сложности на изготовления станка ушёл один месяц.</p><p> </p><p>
Фотки поэтапного изготовления:</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-26804100-1391876622.jpg" data-fileid="29452" data-fileext="jpg" rel=""><img data-fileid="29452" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-26804100-1391876622_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-26804100-1391876622_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-90803600-1391876642.jpg" data-fileid="29454" data-fileext="jpg" rel=""><img data-fileid="29454" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-90803600-1391876642_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-90803600-1391876642_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-53256400-1391876657.jpg" data-fileid="29455" data-fileext="jpg" rel=""><img data-fileid="29455" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-53256400-1391876657_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-53256400-1391876657_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-50104400-1391876675.jpg" data-fileid="29456" data-fileext="jpg" rel=""><img data-fileid="29456" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-50104400-1391876675_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-50104400-1391876675_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-89092100-1391876687.jpg" data-fileid="29457" data-fileext="jpg" rel=""><img data-fileid="29457" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-89092100-1391876687_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-89092100-1391876687_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-59845800-1391876703.jpg" data-fileid="29458" data-fileext="jpg" rel=""><img data-fileid="29458" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-59845800-1391876703_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-59845800-1391876703_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-63868500-1391876725.jpg" data-fileid="29459" data-fileext="jpg" rel=""><img data-fileid="29459" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-63868500-1391876725_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-63868500-1391876725_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-77763700-1391876748.jpg" data-fileid="29460" data-fileext="jpg" rel=""><img data-fileid="29460" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-77763700-1391876748_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-77763700-1391876748_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-08012700-1391876772.jpg" data-fileid="29461" data-fileext="jpg" rel=""><img data-fileid="29461" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-08012700-1391876772_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-08012700-1391876772_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-85518600-1391876796.jpg" data-fileid="29462" data-fileext="jpg" rel=""><img data-fileid="29462" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-85518600-1391876796_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-85518600-1391876796_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-74622800-1391876812.jpg" data-fileid="29463" data-fileext="jpg" rel=""><img data-fileid="29463" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-74622800-1391876812_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-74622800-1391876812_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-29817000-1391876838.jpg" data-fileid="29464" data-fileext="jpg" rel=""><img data-fileid="29464" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-29817000-1391876838_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-29817000-1391876838_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-42681900-1391876863.jpg" data-fileid="29465" data-fileext="jpg" rel=""><img data-fileid="29465" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-42681900-1391876863_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-42681900-1391876863_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-52300900-1391876888.jpg" data-fileid="29466" data-fileext="jpg" rel=""><img data-fileid="29466" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-52300900-1391876888_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-52300900-1391876888_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-55810100-1391876911.jpg" data-fileid="29467" data-fileext="jpg" rel=""><img data-fileid="29467" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-55810100-1391876911_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-55810100-1391876911_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-29876300-1391876930.jpg" data-fileid="29468" data-fileext="jpg" rel=""><img data-fileid="29468" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-29876300-1391876930_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-29876300-1391876930_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-39529600-1391876951.jpg" data-fileid="29469" data-fileext="jpg" rel=""><img data-fileid="29469" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-39529600-1391876951_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-39529600-1391876951_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-80087300-1391876969.jpg" data-fileid="29470" data-fileext="jpg" rel=""><img data-fileid="29470" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-80087300-1391876969_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-80087300-1391876969_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-34986100-1391876985.jpg" data-fileid="29471" data-fileext="jpg" rel=""><img data-fileid="29471" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-34986100-1391876985_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-34986100-1391876985_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-12632000-1391877004.jpg" data-fileid="29472" data-fileext="jpg" rel=""><img data-fileid="29472" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-12632000-1391877004_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-12632000-1391877004_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-17034100-1391877024.jpg" data-fileid="29473" data-fileext="jpg" rel=""><img data-fileid="29473" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-17034100-1391877024_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-17034100-1391877024_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-21503800-1391877055.jpg" data-fileid="29474" data-fileext="jpg" rel=""><img data-fileid="29474" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-21503800-1391877055_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-21503800-1391877055_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-08674300-1391877096.jpg" data-fileid="29475" data-fileext="jpg" rel=""><img data-fileid="29475" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-08674300-1391877096_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-08674300-1391877096_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-28321700-1391877147.jpg" data-fileid="29477" data-fileext="jpg" rel=""><img data-fileid="29477" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-28321700-1391877147_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-28321700-1391877147_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-59449000-1391877206.jpg" data-fileid="29478" data-fileext="jpg" rel=""><img data-fileid="29478" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-59449000-1391877206_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-59449000-1391877206_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-60600200-1391877251.jpg" data-fileid="29479" data-fileext="jpg" rel=""><img data-fileid="29479" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-60600200-1391877251_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-60600200-1391877251_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-54800600-1391877326.jpg" data-fileid="29481" data-fileext="jpg" rel=""><img data-fileid="29481" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-54800600-1391877326_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-54800600-1391877326_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-87690300-1391877369.jpg" data-fileid="29482" data-fileext="jpg" rel=""><img data-fileid="29482" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-87690300-1391877369_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-87690300-1391877369_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-04935700-1391877397.jpg" data-fileid="29483" data-fileext="jpg" rel=""><img data-fileid="29483" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-04935700-1391877397_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-04935700-1391877397_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-71910200-1391877423.jpg" data-fileid="29484" data-fileext="jpg" rel=""><img data-fileid="29484" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-71910200-1391877423_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-71910200-1391877423_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-99684900-1391877446.jpg" data-fileid="29485" data-fileext="jpg" rel=""><img data-fileid="29485" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-99684900-1391877446_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-99684900-1391877446_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-32082800-1391877480.jpg" data-fileid="29486" data-fileext="jpg" rel=""><img data-fileid="29486" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-32082800-1391877480_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-32082800-1391877480_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-08099600-1391877505.jpg" data-fileid="29487" data-fileext="jpg" rel=""><img data-fileid="29487" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-08099600-1391877505_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-08099600-1391877505_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-95360500-1391877526.jpg" data-fileid="29488" data-fileext="jpg" rel=""><img data-fileid="29488" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-95360500-1391877526_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-95360500-1391877526_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-50694500-1391877553.jpg" data-fileid="29489" data-fileext="jpg" rel=""><img data-fileid="29489" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-50694500-1391877553_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-50694500-1391877553_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-69021700-1391882203.jpg" data-fileid="29504" data-fileext="jpg" rel=""><img data-fileid="29504" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-69021700-1391882203_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-69021700-1391882203_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-22236200-1391882238.jpg" data-fileid="29505" data-fileext="jpg" rel=""><img data-fileid="29505" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-22236200-1391882238_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-22236200-1391882238_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-54924000-1391882254.jpg" data-fileid="29506" data-fileext="jpg" rel=""><img data-fileid="29506" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-54924000-1391882254_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-54924000-1391882254_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-15926100-1391882300.jpg" data-fileid="29507" data-fileext="jpg" rel=""><img data-fileid="29507" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-15926100-1391882300_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-15926100-1391882300_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-99369400-1391882358.jpg" data-fileid="29508" data-fileext="jpg" rel=""><img data-fileid="29508" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-99369400-1391882358_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-99369400-1391882358_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-22740500-1391882382.jpg" data-fileid="29509" data-fileext="jpg" rel=""><img data-fileid="29509" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-22740500-1391882382_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-22740500-1391882382_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-46627200-1391882421.jpg" data-fileid="29510" data-fileext="jpg" rel=""><img data-fileid="29510" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-46627200-1391882421_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-46627200-1391882421_thumb.jpg"></a></p><p> </p><p> </p><p>
<strong>Стойка для радиаторов</strong></p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-44212600-1391921701.jpg" data-fileid="29587" data-fileext="jpg" rel=""><img data-fileid="29587" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-44212600-1391921701_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-44212600-1391921701_thumb.jpg"></a></p><p> </p><p>
Когда нет сил ворочить тяжеленные радиаторы, то такая стойка значительно упрощает это занятие.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-89221900-1391921223.jpg" data-fileid="29574" data-fileext="jpg" rel=""><img data-fileid="29574" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-89221900-1391921223_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-89221900-1391921223_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-25652900-1391921259.jpg" data-fileid="29575" data-fileext="jpg" rel=""><img data-fileid="29575" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-25652900-1391921259_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-25652900-1391921259_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-43923100-1391921323.jpg" data-fileid="29576" data-fileext="jpg" rel=""><img data-fileid="29576" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-43923100-1391921323_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-43923100-1391921323_thumb.jpg"></a></p><p> </p><p>
Элементы конструкции и крепления к подъемнику</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-17161200-1391921360.jpg" data-fileid="29578" data-fileext="jpg" rel=""><img data-fileid="29578" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-17161200-1391921360_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-17161200-1391921360_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-52437900-1391921402.jpg" data-fileid="29579" data-fileext="jpg" rel=""><img data-fileid="29579" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-52437900-1391921402_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-52437900-1391921402_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-18288600-1391921432.jpg" data-fileid="29580" data-fileext="jpg" rel=""><img data-fileid="29580" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-18288600-1391921432_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-18288600-1391921432_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-49156700-1391921449.jpg" data-fileid="29581" data-fileext="jpg" rel=""><img data-fileid="29581" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-49156700-1391921449_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-49156700-1391921449_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-67837500-1391921464.jpg" data-fileid="29582" data-fileext="jpg" rel=""><img data-fileid="29582" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-67837500-1391921464_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-67837500-1391921464_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-66374100-1391921490.jpg" data-fileid="29583" data-fileext="jpg" rel=""><img data-fileid="29583" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-66374100-1391921490_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-66374100-1391921490_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-87620600-1391921514.jpg" data-fileid="29584" data-fileext="jpg" rel=""><img data-fileid="29584" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-87620600-1391921514_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-87620600-1391921514_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-47050900-1391921530.jpg" data-fileid="29585" data-fileext="jpg" rel=""><img data-fileid="29585" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-47050900-1391921530_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-47050900-1391921530_thumb.jpg"></a></p><p> </p><p>
Если она мешает, то монтаж и демонтаж стойки производится в течении одной минуты.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-34637100-1391921555.jpg" data-fileid="29586" data-fileext="jpg" rel=""><img data-fileid="29586" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-34637100-1391921555_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-34637100-1391921555_thumb.jpg"></a></p><p> </p><p> </p><p>
<strong>Подъёмник</strong></p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1-0-87257400-1392113959.jpg" data-fileid="29815" data-fileext="jpg" rel=""><img data-fileid="29815" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-87257400-1392113959_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1-0-87257400-1392113959_thumb.jpg"></a></p><p> </p><p>
Подъёмник изготавливался давненько, и из того что было, специально ничего не покупалось. До сих пор служит мне исправно. <img alt=":friends:" src="https://websvarka.ru/talk/uploads/emoticons/default_friends.gif"></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-35224600-1391920576.jpg" data-fileid="29568" data-fileext="jpg" rel=""><img data-fileid="29568" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-35224600-1391920576_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-35224600-1391920576_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-36982000-1391920436.jpg" data-fileid="29566" data-fileext="jpg" rel=""><img data-fileid="29566" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-36982000-1391920436_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-36982000-1391920436_thumb.jpg"></a></p><p> </p><p>
Вид снизу</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-69484500-1391919657.jpg" data-fileid="29557" data-fileext="jpg" rel=""><img data-fileid="29557" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-69484500-1391919657_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-69484500-1391919657_thumb.jpg"></a></p><p> </p><p>
Ножничный узел</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-09369400-1391919616.jpg" data-fileid="29554" data-fileext="jpg" rel=""><img data-fileid="29554" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-09369400-1391919616_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-09369400-1391919616_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-04404800-1391920707.jpg" data-fileid="29570" data-fileext="jpg" rel=""><img data-fileid="29570" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-04404800-1391920707_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-04404800-1391920707_thumb.jpg"></a></p><p> </p><p>
Катки верхние и нижние</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-69267300-1391919625.jpg" data-fileid="29555" data-fileext="jpg" rel=""><img data-fileid="29555" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-69267300-1391919625_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-69267300-1391919625_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-19255800-1391919608.jpg" data-fileid="29553" data-fileext="jpg" rel=""><img data-fileid="29553" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-19255800-1391919608_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-19255800-1391919608_thumb.jpg"></a></p><p> </p><p>
Шарнирный узел</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-29309900-1391919667.jpg" data-fileid="29558" data-fileext="jpg" rel=""><img data-fileid="29558" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-29309900-1391919667_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-29309900-1391919667_thumb.jpg"></a></p><p> </p><p>
Крепление гидроцилиндров</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-01775000-1391919639.jpg" data-fileid="29556" data-fileext="jpg" rel=""><img data-fileid="29556" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-01775000-1391919639_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-01775000-1391919639_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-15798700-1391919683.jpg" data-fileid="29560" data-fileext="jpg" rel=""><img data-fileid="29560" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-15798700-1391919683_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-15798700-1391919683_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-15377200-1391920673.jpg" data-fileid="29569" data-fileext="jpg" rel=""><img data-fileid="29569" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-15377200-1391920673_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-15377200-1391920673_thumb.jpg"></a></p><p> </p><p>
И моя гидростанция для подъёмника</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-83222000-1391919596.jpg" data-fileid="29551" data-fileext="jpg" rel=""><img data-fileid="29551" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-83222000-1391919596_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-83222000-1391919596_thumb.jpg"></a></p><p> </p><p> </p><p>
<strong>Трактор</strong></p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-49227900-1391925032.jpg" data-fileid="29607" data-fileext="jpg" rel=""><img data-fileid="29607" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-49227900-1391925032_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-49227900-1391925032_thumb.jpg"></a></p><p> </p><p>
А это был мой незаменимый помощник, сделаный специально для строительства дома. Для грейдирования участка, перевозки сыпучих грузов и пиломатериала длиной до 8 метров. Сделал я его в 1995 году. На постройку ушёл весь отпуск, ну и полгода предшествовала подготовка к постройке (обрезка мостов, поиск запчастей и т.п.). Движка ВАЗ 2105 с КПП+КПП ЗИЛ 130.</p><p> </p><p>
Передний мост УАЗ, задний ГАЗ 51. Привод переднего моста от коробки отбора мощности ЗИЛ 130. Фоток поэтапного строительства нет, т.к тогда даже фотика не было. Потом дополнительно изготовил плуг и автономную косилку. В 2010 году трактор был продан к деревню и до сих пор служит исправно.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-73521300-1391924435.jpg" data-fileid="29596" data-fileext="jpg" rel=""><img data-fileid="29596" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-73521300-1391924435_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-73521300-1391924435_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-40988300-1391924815.jpg" data-fileid="29597" data-fileext="jpg" rel=""><img data-fileid="29597" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-40988300-1391924815_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-40988300-1391924815_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-00594500-1391924860.jpg" data-fileid="29599" data-fileext="jpg" rel=""><img data-fileid="29599" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-00594500-1391924860_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-00594500-1391924860_thumb.jpg"></a></p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-38295400-1391924843.jpg" data-fileid="29598" data-fileext="jpg" rel=""><img data-fileid="29598" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-38295400-1391924843_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-38295400-1391924843_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-48979700-1391924873.jpg" data-fileid="29600" data-fileext="jpg" rel=""><img data-fileid="29600" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-48979700-1391924873_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-48979700-1391924873_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-29526400-1391924901.jpg" data-fileid="29601" data-fileext="jpg" rel=""><img data-fileid="29601" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-29526400-1391924901_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-29526400-1391924901_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-41662200-1391924915.jpg" data-fileid="29602" data-fileext="jpg" rel=""><img data-fileid="29602" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-41662200-1391924915_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-41662200-1391924915_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-74866000-1391924928.jpg" data-fileid="29603" data-fileext="jpg" rel=""><img data-fileid="29603" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-74866000-1391924928_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-74866000-1391924928_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-06083800-1391924950.jpg" data-fileid="29604" data-fileext="jpg" rel=""><img data-fileid="29604" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-06083800-1391924950_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-06083800-1391924950_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-56163700-1391924973.jpg" data-fileid="29605" data-fileext="jpg" rel=""><img data-fileid="29605" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-56163700-1391924973_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-56163700-1391924973_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-33483200-1391925051.jpg" data-fileid="29608" data-fileext="jpg" rel=""><img data-fileid="29608" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-33483200-1391925051_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-33483200-1391925051_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-66822000-1391925116.jpg" data-fileid="29609" data-fileext="jpg" rel=""><img data-fileid="29609" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-66822000-1391925116_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-66822000-1391925116_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-57209600-1391925008.jpg" data-fileid="29606" data-fileext="jpg" rel=""><img data-fileid="29606" class="ipsImage ipsImage_thumbnailed" alt="post-3288-0-57209600-1391925008_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3288-0-57209600-1391925008_thumb.jpg"></a></p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа № 46</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3851</guid><pubDate>Tue, 11 Feb 2014 13:19:55 +0000</pubDate></item><item><title>&#x411;&#x43B;&#x43E;&#x43A; &#x446;&#x438;&#x43B;&#x438;&#x43D;&#x434;&#x440;&#x43E;&#x432; &#x43E;&#x442; &#x430;&#x432;&#x442;&#x43E;&#x43C;&#x43E;&#x431;&#x438;&#x43B;&#x44F; Suzuki</title><link>https://websvarka.ru/talk/topic/3706-blok-tsilindrov-ot-avtomobilya-suzuki/</link><description><![CDATA[
<p>Всем привет. Зовут меня Сергей, хочу предоставить работу по Блоку цилиндров (в дальнейшем БЦ) от автомобиля Suzuki.</p><p>
 </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-49277400-1390494362.jpg" data-fileid="27777" data-fileext="jpg" rel=""><img data-fileid="27777" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-49277400-1390494362_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-49277400-1390494362_thumb.jpg"></a></p><p>
 </p><p>
Я постарался сделать снимки, показывающие последовательность выполняемых работ.</p><p>
 </p><p>
Ниже на первых двух снимках показан БЦ с двух сторон. После опрессовки красным помечены трещины, откуда вытекает охлаждающая жидкость. Вырваны столбы (сливной масляный канал и резьбовое отверстие крепления головки).</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-54985000-1390493196.jpg" data-fileid="27758" data-fileext="jpg" rel=""><img data-fileid="27758" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-54985000-1390493196_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-54985000-1390493196_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-06521300-1390493213.jpg" data-fileid="27759" data-fileext="jpg" rel=""><img data-fileid="27759" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-06521300-1390493213_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-06521300-1390493213_thumb.jpg"></a></p><p>
 </p><p>
Точно причину назвать трудно: перетянули (тянули с другим моментом затяжки), попала жидкость в резьбовой канал или заводской брак литья к примеру. Многие варят по наружи БЦ и отдают. Мы же понимаем, что нам нужно добраться до последней (третей) стенки резьбового канала, который внутри блока около самих цилиндров. Поэтому отложим пока горелку (часов на 6) и возьмем дрель и шарошку <img alt=":rolleyes:" src="https://websvarka.ru/talk/uploads/emoticons/default_rolleyes.gif">.</p><p>
 </p><p>
Начало разделки. Если хорошо приглядеться, можно увидеть трещину.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-88327100-1390494141.jpg" data-fileid="27762" data-fileext="jpg" rel=""><img data-fileid="27762" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-88327100-1390494141_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-88327100-1390494141_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-78494600-1390494153.jpg" data-fileid="27763" data-fileext="jpg" rel=""><img data-fileid="27763" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-78494600-1390494153_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-78494600-1390494153_thumb.jpg"></a></p><p> </p><p>
БЦ с обеих сторон зачищен под сварку:</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-76683500-1390494166.jpg" data-fileid="27764" data-fileext="jpg" rel=""><img data-fileid="27764" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-76683500-1390494166_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-76683500-1390494166_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-45275700-1390494182.jpg" data-fileid="27765" data-fileext="jpg" rel=""><img data-fileid="27765" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-45275700-1390494182_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-45275700-1390494182_thumb.jpg"></a></p><p>
 </p><p>
«Выварка» рубашки охлаждения и первой стенки (резьбового канала) и опрессовка (проверка мелом на керосин) герметичности. </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-99551100-1390494196.jpg" data-fileid="27766" data-fileext="jpg" rel=""><img data-fileid="27766" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-99551100-1390494196_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-99551100-1390494196_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-63707200-1390494212.jpg" data-fileid="27767" data-fileext="jpg" rel=""><img data-fileid="27767" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-63707200-1390494212_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-63707200-1390494212_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-55332500-1390494227.jpg" data-fileid="27768" data-fileext="jpg" rel=""><img data-fileid="27768" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-55332500-1390494227_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-55332500-1390494227_thumb.jpg"></a></p><p> </p><p>
Печь, в которой перед сваркой подогревается блок (примерно с этой работой грелся и остывал он раз 5).</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-64806100-1390494239.jpg" data-fileid="27769" data-fileext="jpg" rel=""><img data-fileid="27769" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-64806100-1390494239_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-64806100-1390494239_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-29641200-1390494257.jpg" data-fileid="27770" data-fileext="jpg" rel=""><img data-fileid="27770" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-29641200-1390494257_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-29641200-1390494257_thumb.jpg"></a></p><p> </p><p>
Дальше следует выварка полностью резьбового канала (остывание блока), и также проверка на герметичность керосином (но льем уже не в рубашку охлаждения, а в резьбовой канал). И потом вывариваем сливной масляный канал и так же проверяем на герметичность.</p><p> </p><p>
Далее заключительные работы — восстановление ребер жесткости и наварка плоскости БЦ (так как естественно у нас все утянуло).</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-24519800-1390494271.jpg" data-fileid="27771" data-fileext="jpg" rel=""><img data-fileid="27771" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-24519800-1390494271_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-24519800-1390494271_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-20234200-1390494289.jpg" data-fileid="27772" data-fileext="jpg" rel=""><img data-fileid="27772" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-20234200-1390494289_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-20234200-1390494289_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-65415900-1390494327.jpg" data-fileid="27774" data-fileext="jpg" rel=""><img data-fileid="27774" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-65415900-1390494327_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-65415900-1390494327_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-76705200-1390494343.jpg" data-fileid="27775" data-fileext="jpg" rel=""><img data-fileid="27775" class="ipsImage ipsImage_thumbnailed" alt="post-10307-0-76705200-1390494343_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-10307-0-76705200-1390494343_thumb.jpg"></a></p><p> </p><p>
На этом мои работы по сварке и восстановлению закончены. Дальше уже будут станочные работы и опрессовка БЦ под давлением в специальной ванне, а после — опрессовка с установленной на БЦ головкой и рекомендованным моментом затяжки.</p><p> </p><p>
Спасибо, что дочитали до конца. Надеюсь, что не особо утомил своей писаниной... и так старался кратко все описать)).</p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа №11</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3706</guid><pubDate>Thu, 23 Jan 2014 17:10:32 +0000</pubDate></item><item><title>&#x410;&#x432;&#x442;&#x43E;&#x43C;&#x43E;&#x431;&#x438;&#x43B;&#x44C;&#x43D;&#x44B;&#x439; &#x440;&#x430;&#x434;&#x438;&#x430;&#x442;&#x43E;&#x440;</title><link>https://websvarka.ru/talk/topic/3658-avtomobilnyy-radiator/</link><description><![CDATA[
<p>Выставляю на суд свои навыки в аргонодуговой сварке, то есть ТIG.</p><p>
 </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-05693000-1390049823.jpg" data-fileid="27434" data-fileext="jpg" rel=""><img data-fileid="27434" class="ipsImage ipsImage_thumbnailed" alt="post-2095-0-05693000-1390049823_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-05693000-1390049823_thumb.jpg"></a></p><p>
 </p><p>
Непрерывный стаж в этом виде сварки около 13 лет. Работы проводятся на проф. оборудовании фирмы ESAB, а так же на сварочном аппарате собственного изготовления, собранном по заводской схеме. Основная моя работа на производстве — это обварка элементов автомобильных радиаторов: масляных (ЗИЛ), интеркулеров (МАЗ, МТЗ, ГАЗ, ЗИЛ), основных охлаждения двигателей (МАЗ, МТЗ), а также радиаторов различного назначения,например: компрессорные (масляные) большого давления, но естественно и бачки тоже обвариваю. После обварки элементов проверка на мел с керосином, т.е. на герметичность.Технология довольно сложная, всего не опишешь — это нужно видеть. Фотографиям нескольких лет. Было видео, но, к сожалению, не сохранилось.</p><p>
 </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-32463100-1390049858.jpg" data-fileid="27435" data-fileext="jpg" rel=""><img data-fileid="27435" class="ipsImage ipsImage_thumbnailed" alt="post-2095-0-32463100-1390049858_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-32463100-1390049858_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-35416800-1390049956.jpg" data-fileid="27436" data-fileext="jpg" rel=""><img data-fileid="27436" class="ipsImage ipsImage_thumbnailed" alt="post-2095-0-35416800-1390049956_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-35416800-1390049956_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-52956700-1390050022.jpg" data-fileid="27437" data-fileext="jpg" rel=""><img data-fileid="27437" class="ipsImage ipsImage_thumbnailed" alt="post-2095-0-52956700-1390050022_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-52956700-1390050022_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-72607300-1390050210.jpg" data-fileid="27438" data-fileext="jpg" rel=""><img data-fileid="27438" class="ipsImage ipsImage_thumbnailed" alt="post-2095-0-72607300-1390050210_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-72607300-1390050210_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-79134600-1390050302.jpg" data-fileid="27439" data-fileext="jpg" rel=""><img data-fileid="27439" class="ipsImage ipsImage_thumbnailed" alt="post-2095-0-79134600-1390050302_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-79134600-1390050302_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-91296700-1390050366.jpg" data-fileid="27440" data-fileext="jpg" rel=""><img data-fileid="27440" class="ipsImage ipsImage_thumbnailed" alt="post-2095-0-91296700-1390050366_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-91296700-1390050366_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-02443400-1390050419.jpg" data-fileid="27441" data-fileext="jpg" rel=""><img data-fileid="27441" class="ipsImage ipsImage_thumbnailed" alt="post-2095-0-02443400-1390050419_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-02443400-1390050419_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-22699600-1390050468.jpg" data-fileid="27442" data-fileext="jpg" rel=""><img data-fileid="27442" class="ipsImage ipsImage_thumbnailed" alt="post-2095-0-22699600-1390050468_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-22699600-1390050468_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-80208600-1390050505.jpg" data-fileid="27443" data-fileext="jpg" rel=""><img data-fileid="27443" class="ipsImage ipsImage_thumbnailed" alt="post-2095-0-80208600-1390050505_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-80208600-1390050505_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-24757100-1390050595.jpg" data-fileid="27445" data-fileext="jpg" rel=""><img data-fileid="27445" class="ipsImage ipsImage_thumbnailed" alt="post-2095-0-24757100-1390050595_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-24757100-1390050595_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-51342000-1390050719.jpg" data-fileid="27447" data-fileext="jpg" rel=""><img data-fileid="27447" class="ipsImage ipsImage_thumbnailed" alt="post-2095-0-51342000-1390050719_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-51342000-1390050719_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-10866800-1390050838.jpg" data-fileid="27448" data-fileext="jpg" rel=""><img data-fileid="27448" class="ipsImage ipsImage_thumbnailed" alt="post-2095-0-10866800-1390050838_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-10866800-1390050838_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-99787400-1390050913.jpg" data-fileid="27449" data-fileext="jpg" rel=""><img data-fileid="27449" class="ipsImage ipsImage_thumbnailed" alt="post-2095-0-99787400-1390050913_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-2095-0-99787400-1390050913_thumb.jpg"></a></p><p>
 </p><p>
</p><hr><p>
<strong>Конкурсная работа №6</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3658</guid><pubDate>Mon, 20 Jan 2014 08:33:39 +0000</pubDate></item><item><title>&#x422;&#x440;&#x435;&#x43D;&#x430;&#x436;&#x435;&#x440;</title><link>https://websvarka.ru/talk/topic/3952-trenazher/</link><description><![CDATA[
<p>Доброго времени суток. Некоторое время занимаюсь металлом. Мастерская у себя в гараже. Закончил тренажер сегодня т.е. 22 февраля.</p><p>
 </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11409-0-85155100-1392996414.jpg" data-fileid="31049" data-fileext="jpg" rel=""><img data-fileid="31049" class="ipsImage ipsImage_thumbnailed" alt="post-11409-0-85155100-1392996414_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11409-0-85155100-1392996414_thumb.jpg"></a></p><p>
 </p><p>
Тренажер называется ЖИМ НОГАМИ ПОД УГЛОМ 45 Градусов. Использовал: металлическая профильная труба 80х40х3, 60х40х3, 40х40х3, 25х25х2, 20х20х1,5, круг 50, 25, труба 25,20,15. швеллер 10, лист 3 мм, лист 5 мм, рифл. алюминий, в качестве роликов — ролики от коньков. Полимерную покраску освоил в прошлом году.</p><p>
 </p><p>
Подготовка к покраске</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11409-0-31518600-1392996696.jpg" data-fileid="31051" data-fileext="jpg" rel=""><img data-fileid="31051" class="ipsImage ipsImage_thumbnailed" alt="post-11409-0-31518600-1392996696_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11409-0-31518600-1392996696_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11409-0-31518600-1392996696.jpg" data-fileid="31051" data-fileext="jpg" rel=""><img data-fileid="31051" class="ipsImage ipsImage_thumbnailed" alt="post-11409-0-31518600-1392996696_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11409-0-31518600-1392996696_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11409-0-30068600-1392997250.jpg" data-fileid="31053" data-fileext="jpg" rel=""><img data-fileid="31053" class="ipsImage ipsImage_thumbnailed" alt="post-11409-0-30068600-1392997250_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11409-0-30068600-1392997250_thumb.jpg"></a></p><p>
 </p><p>
Все готово</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11409-0-27659200-1392996547.jpg" data-fileid="31050" data-fileext="jpg" rel=""><img data-fileid="31050" class="ipsImage ipsImage_thumbnailed" alt="post-11409-0-27659200-1392996547_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11409-0-27659200-1392996547_thumb.jpg"></a></p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа № 74</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3952</guid><pubDate>Fri, 21 Feb 2014 15:42:08 +0000</pubDate></item><item><title>&#x41C;&#x43E;&#x431;&#x438;&#x43B;&#x44C;&#x43D;&#x44B;&#x439; &#x433;&#x43E;&#x440;&#x43D;&#x43E;&#x43B;&#x44B;&#x436;&#x43D;&#x44B;&#x439; &#x43F;&#x43E;&#x434;&#x44A;&#x451;&#x43C;&#x43D;&#x438;&#x43A;</title><link>https://websvarka.ru/talk/topic/3898-mobilnyy-gornolyzhnyy-podyomnik/</link><description><![CDATA[
<p>Приветствую! До этого молчал как партизан ибо работы было много и некогда было забрать последние детали из покраски. Итак на суд общественности предоставляется бензиновая версия малого мобильного горнолыжного подъёмника.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7662-0-02345800-1392452855.jpg" data-fileid="30167" data-fileext="jpg" rel=""><img data-fileid="30167" class="ipsImage ipsImage_thumbnailed" alt="post-7662-0-02345800-1392452855_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7662-0-02345800-1392452855_thumb.jpg"></a></p><p> </p><p>
Габаритные размеры изделия таковы, что в разобранном состоянии все помещается в багажник Volkswagen Golf.</p><p>
Масса приводной станции — 62 кг (мотор редуктор + рама + двигатель + шкив)/</p><p>
Общая масса всех составных частей с 220 метрами 16 мм троса — 120 кг.</p><p>
На видео используется тестовый отрезок 12 мм троса.</p><p>
Расчетное натяжение троса — 600 кг.</p><p>
 </p><p>
<a href="http://www.youtube.com/watch?v=ZqDOGh8MTT4" rel="external nofollow">http://www.youtube.com/watch?v=ZqDOGh8MTT4</a></p><p> </p><p>
На видео не установлены преднатяжители и выравниватель положения шкивов (регулируют от +25 до -25 градусов от горизонтали).</p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа № 59</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3898</guid><pubDate>Mon, 17 Feb 2014 09:39:10 +0000</pubDate></item><item><title>&#x421;&#x435;&#x440;&#x438;&#x44F; &#x434;&#x432;&#x435;&#x440;&#x43D;&#x44B;&#x445; &#x440;&#x443;&#x447;&#x435;&#x43A;</title><link>https://websvarka.ru/talk/topic/3908-seriya-dvernyh-ruchek/</link><description><![CDATA[
<p>Здравствуйте! На форуме я новичок, зашел сюда в поисках конструкции печки для мастерской. Три года назад ушел с головой в работу с металлом, сварка и ковка. Делаю, в основном, интерьерные вещи: мебель, светильники, небольшие скульптуры, фигурки в стиле техноарт из болтов и шурупов. Представленные дверные ручки выполнены из обрезков труб и листового металла. Фактуру наносил сваркой и ковкой.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-96493300-1392562275.jpg" data-fileid="30379" data-fileext="jpg" rel=""><img data-fileid="30379" class="ipsImage ipsImage_thumbnailed" alt="post-11352-0-96493300-1392562275_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-96493300-1392562275_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-67586200-1392562501.jpg" data-fileid="30384" data-fileext="jpg" rel=""><img data-fileid="30384" class="ipsImage ipsImage_thumbnailed" alt="post-11352-0-67586200-1392562501_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-67586200-1392562501_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-56622900-1392562466.jpg" data-fileid="30383" data-fileext="jpg" rel=""><img data-fileid="30383" class="ipsImage ipsImage_thumbnailed" alt="post-11352-0-56622900-1392562466_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-56622900-1392562466_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-71571200-1392562703.jpg" data-fileid="30389" data-fileext="jpg" rel=""><img data-fileid="30389" class="ipsImage ipsImage_thumbnailed" alt="post-11352-0-71571200-1392562703_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-71571200-1392562703_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-13441300-1392562527.jpg" data-fileid="30385" data-fileext="jpg" rel=""><img data-fileid="30385" class="ipsImage ipsImage_thumbnailed" alt="post-11352-0-13441300-1392562527_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-13441300-1392562527_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-52003600-1392562557.jpg" data-fileid="30386" data-fileext="jpg" rel=""><img data-fileid="30386" class="ipsImage ipsImage_thumbnailed" alt="post-11352-0-52003600-1392562557_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-52003600-1392562557_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-38157200-1392562581.jpg" data-fileid="30387" data-fileext="jpg" rel=""><img data-fileid="30387" class="ipsImage ipsImage_thumbnailed" alt="post-11352-0-38157200-1392562581_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-38157200-1392562581_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-81172400-1392562627.jpg" data-fileid="30388" data-fileext="jpg" rel=""><img data-fileid="30388" class="ipsImage ipsImage_thumbnailed" alt="post-11352-0-81172400-1392562627_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-81172400-1392562627_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-73899600-1392562432.jpg" data-fileid="30382" data-fileext="jpg" rel=""><img data-fileid="30382" class="ipsImage ipsImage_thumbnailed" alt="post-11352-0-73899600-1392562432_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11352-0-73899600-1392562432_thumb.jpg"></a></p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа № 61</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3908</guid><pubDate>Mon, 17 Feb 2014 13:19:11 +0000</pubDate></item><item><title>&#x41F;&#x440;&#x438;&#x446;&#x435;&#x43F;&#x44B; &#x434;&#x43B;&#x44F; &#x432;&#x43D;&#x435;&#x434;&#x43E;&#x440;&#x43E;&#x436;&#x43D;&#x438;&#x43A;&#x43E;&#x432;</title><link>https://websvarka.ru/talk/topic/3791-pritsepy-dlya-vnedorozhnikov/</link><description><![CDATA[
<p>Приветствую! Меня зовут Антон Лазуренко. Я обитаю в Москве и занимаюсь тюнингом различных средств передвижения, а с недавних пор еще и реставрацией классических автомобилей и кастомайзингом. У меня накоплено немало работ разного направления и стилей, которые я создал, работая в различных мастерских. Но мне показалось, что для аудитории, собравшейся на этом сайте, будет интересна тема внедорожников, рыбалки и путешествий.</p><p> </p><p>
Работы, которые хочу представить вашему вниманию, были выполнены мной в одной из мастерских по тюнингу внедорожников в 2012-2013 гг. Идеи всех этих прицепов принадлежат не мне одному. Концепции рождались при общении с клиентами. Никаких предварительных расчетов никто не производил. Клиент объяснял, что он хочет видеть, а как это реализовать приходилось придумывать самому.</p><p> </p><p>
Работать я люблю один и поэтому к сторонней помощи прибегал крайне редко. Все, что потребовалось для создания этих прицепов — это сварочный полуавтомат, балгарка, дрель, набор ключей, рулетка и немного фантазии <img alt=":)" src="https://websvarka.ru/talk/uploads/emoticons/default_smile.png"></p><p>
 </p><p>
<strong>Прицеп для катера</strong></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-42526400-1391282331.jpg" data-fileid="28691" data-fileext="jpg" rel=""><img data-fileid="28691" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-42526400-1391282331_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-42526400-1391282331_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-97179700-1391282722.jpg" data-fileid="28698" data-fileext="jpg" rel=""><img data-fileid="28698" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-97179700-1391282722_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-97179700-1391282722_thumb.jpg"></a></p><p> </p><p>
Здесь стояла задача добавить жесткость раме и сделать ступеньки для удобства при перевозке.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-29478100-1391282517.jpg" data-fileid="28694" data-fileext="jpg" rel=""><img data-fileid="28694" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-29478100-1391282517_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-29478100-1391282517_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-93931900-1391282436.jpg" data-fileid="28693" data-fileext="jpg" rel=""><img data-fileid="28693" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-93931900-1391282436_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-93931900-1391282436_thumb.jpg"></a></p><p> </p><p>
Добавляем функционал. Крепление запасного колеса.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-46028400-1391282524.jpg" data-fileid="28695" data-fileext="jpg" rel=""><img data-fileid="28695" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-46028400-1391282524_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-46028400-1391282524_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-84385300-1391282536.jpg" data-fileid="28696" data-fileext="jpg" rel=""><img data-fileid="28696" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-84385300-1391282536_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-84385300-1391282536_thumb.jpg"></a></p><p> </p><p>
Зашивать ступеньки будем рифленым алюминием.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-44720100-1391282625.jpg" data-fileid="28697" data-fileext="jpg" rel=""><img data-fileid="28697" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-44720100-1391282625_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-44720100-1391282625_thumb.jpg"></a></p><p> </p><p>
Все детали покрыты порошковой краской.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-66336000-1391282731.jpg" data-fileid="28699" data-fileext="jpg" rel=""><img data-fileid="28699" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-66336000-1391282731_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-66336000-1391282731_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-34735500-1391282740.jpg" data-fileid="28700" data-fileext="jpg" rel=""><img data-fileid="28700" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-34735500-1391282740_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-34735500-1391282740_thumb.jpg"></a></p><p>
 </p><p>
<strong>Прицеп фургон</strong></p><p>
Здесь все просто. Клиент пожелал вместительный прицеп для снаряжения. Основа — заводская рама. На ней изготовил металлическую будку.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-55357600-1391283127.jpg" data-fileid="28702" data-fileext="jpg" rel=""><img data-fileid="28702" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-55357600-1391283127_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-55357600-1391283127_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-85012700-1391283131.jpg" data-fileid="28703" data-fileext="jpg" rel=""><img data-fileid="28703" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-85012700-1391283131_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-85012700-1391283131_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-42291000-1391283136.jpg" data-fileid="28704" data-fileext="jpg" rel=""><img data-fileid="28704" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-42291000-1391283136_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-42291000-1391283136_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-52830200-1391283146.jpg" data-fileid="28706" data-fileext="jpg" rel=""><img data-fileid="28706" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-52830200-1391283146_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-52830200-1391283146_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-28604800-1391283140.jpg" data-fileid="28705" data-fileext="jpg" rel=""><img data-fileid="28705" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-28604800-1391283140_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-28604800-1391283140_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-62214300-1391283150.jpg" data-fileid="28707" data-fileext="jpg" rel=""><img data-fileid="28707" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-62214300-1391283150_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-62214300-1391283150_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-54477200-1391283121.jpg" data-fileid="28701" data-fileext="jpg" rel=""><img data-fileid="28701" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-54477200-1391283121_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-54477200-1391283121_thumb.jpg"></a></p><p> </p><p>
После покраски и сборки получился вот такой грузовик.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-35972900-1391283345.jpg" data-fileid="28711" data-fileext="jpg" rel=""><img data-fileid="28711" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-35972900-1391283345_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-35972900-1391283345_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-38642000-1391283337.jpg" data-fileid="28710" data-fileext="jpg" rel=""><img data-fileid="28710" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-38642000-1391283337_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-38642000-1391283337_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-04235400-1391283325.jpg" data-fileid="28708" data-fileext="jpg" rel=""><img data-fileid="28708" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-04235400-1391283325_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-04235400-1391283325_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-81540800-1391283330.jpg" data-fileid="28709" data-fileext="jpg" rel=""><img data-fileid="28709" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-81540800-1391283330_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-81540800-1391283330_thumb.jpg"></a></p><p>
 </p><p>
<strong>Прицеп для рыбака</strong></p><p>
Этот проект интереснее. Здесь заложен довольно большой функционал:</p><p>
- перевозка надувной лодки в надутом состоянии,</p><p>
- перевозка лодочного мотора,</p><p>
- двухместная палатка на крыше,</p><p>
- кухня с газовой плитой и раковиной,</p><p>
- душ.</p><p> </p><p>
Основа — заводская рама. На ней делаем основной грузовой отсек с боковыми ящиками.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-36638500-1391283818.jpg" data-fileid="28713" data-fileext="jpg" rel=""><img data-fileid="28713" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-36638500-1391283818_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-36638500-1391283818_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-90080700-1391284347.jpg" data-fileid="28723" data-fileext="jpg" rel=""><img data-fileid="28723" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-90080700-1391284347_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-90080700-1391284347_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-68269500-1391283822.jpg" data-fileid="28714" data-fileext="jpg" rel=""><img data-fileid="28714" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-68269500-1391283822_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-68269500-1391283822_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-91825500-1391283826.jpg" data-fileid="28715" data-fileext="jpg" rel=""><img data-fileid="28715" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-91825500-1391283826_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-91825500-1391283826_thumb.jpg"></a></p><p> </p><p>
Стандартное дышло заменено на мощное немецкое. Чтобы его установить, нужно было сделать новые крепления.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-97691800-1391283935.jpg" data-fileid="28716" data-fileext="jpg" rel=""><img data-fileid="28716" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-97691800-1391283935_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-97691800-1391283935_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-69446200-1391283948.jpg" data-fileid="28717" data-fileext="jpg" rel=""><img data-fileid="28717" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-69446200-1391283948_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-69446200-1391283948_thumb.jpg"></a></p><p> </p><p>
Сзади будет перевозиться лодочный мотор или запасное колесо. Изготовил калитку.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-04415900-1391284153.jpg" data-fileid="28721" data-fileext="jpg" rel=""><img data-fileid="28721" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-04415900-1391284153_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-04415900-1391284153_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-79568500-1391284148.jpg" data-fileid="28720" data-fileext="jpg" rel=""><img data-fileid="28720" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-79568500-1391284148_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-79568500-1391284148_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-79025600-1391284142.jpg" data-fileid="28719" data-fileext="jpg" rel=""><img data-fileid="28719" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-79025600-1391284142_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-79025600-1391284142_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-93824700-1391284156.jpg" data-fileid="28722" data-fileext="jpg" rel=""><img data-fileid="28722" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-93824700-1391284156_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-93824700-1391284156_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-88256000-1391284137.jpg" data-fileid="28718" data-fileext="jpg" rel=""><img data-fileid="28718" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-88256000-1391284137_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-88256000-1391284137_thumb.jpg"></a></p><p> </p><p>
Защита крыльев , она же удобная ступенька.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-68325200-1391284433.jpg" data-fileid="28724" data-fileext="jpg" rel=""><img data-fileid="28724" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-68325200-1391284433_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-68325200-1391284433_thumb.jpg"></a></p><p> </p><p>
Предусмотрено место для канистр с топливом или водой.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-10724000-1391284486.jpg" data-fileid="28725" data-fileext="jpg" rel=""><img data-fileid="28725" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-10724000-1391284486_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-10724000-1391284486_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-65304100-1391284489.jpg" data-fileid="28726" data-fileext="jpg" rel=""><img data-fileid="28726" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-65304100-1391284489_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-65304100-1391284489_thumb.jpg"></a></p><p> </p><p>
На верхней крышке грузового отсека установлена палатка.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-35818200-1391284604.jpg" data-fileid="28727" data-fileext="jpg" rel=""><img data-fileid="28727" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-35818200-1391284604_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-35818200-1391284604_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-00027500-1391284608.jpg" data-fileid="28728" data-fileext="jpg" rel=""><img data-fileid="28728" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-00027500-1391284608_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-00027500-1391284608_thumb.jpg"></a></p><p> </p><p>
Снизу установлен бак для воды на 70 литров.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-15999600-1391284742.jpg" data-fileid="28729" data-fileext="jpg" rel=""><img data-fileid="28729" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-15999600-1391284742_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-15999600-1391284742_thumb.jpg"></a></p><p> </p><p>
Кухонный модуль с дополнительным столиком и газовой плитой.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-09416100-1391284892.jpg" data-fileid="28733" data-fileext="jpg" rel=""><img data-fileid="28733" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-09416100-1391284892_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-09416100-1391284892_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-86839700-1391284887.jpg" data-fileid="28732" data-fileext="jpg" rel=""><img data-fileid="28732" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-86839700-1391284887_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-86839700-1391284887_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-62961000-1391284878.jpg" data-fileid="28731" data-fileext="jpg" rel=""><img data-fileid="28731" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-62961000-1391284878_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-62961000-1391284878_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-24129600-1391284850.jpg" data-fileid="28730" data-fileext="jpg" rel=""><img data-fileid="28730" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-24129600-1391284850_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-24129600-1391284850_thumb.jpg"></a></p><p> </p><p>
Порошковая покраска. Сборка. Сдача проекта.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-53489600-1391285108.jpg" data-fileid="28735" data-fileext="jpg" rel=""><img data-fileid="28735" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-53489600-1391285108_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-53489600-1391285108_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-23511400-1391285098.jpg" data-fileid="28734" data-fileext="jpg" rel=""><img data-fileid="28734" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-23511400-1391285098_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-23511400-1391285098_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-76117300-1391285124.jpg" data-fileid="28738" data-fileext="jpg" rel=""><img data-fileid="28738" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-76117300-1391285124_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-76117300-1391285124_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-24218000-1391285115.jpg" data-fileid="28736" data-fileext="jpg" rel=""><img data-fileid="28736" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-24218000-1391285115_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-24218000-1391285115_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-72818700-1391285129.jpg" data-fileid="28739" data-fileext="jpg" rel=""><img data-fileid="28739" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-72818700-1391285129_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-72818700-1391285129_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-18135600-1391285120.jpg" data-fileid="28737" data-fileext="jpg" rel=""><img data-fileid="28737" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-18135600-1391285120_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-18135600-1391285120_thumb.jpg"></a></p><p>
 </p><p>
<strong>Туристический прицеп</strong></p><p>
К созданию этого прицепа подошли более технологично. По моим размерам на заводе создали трехмерную модель прицепа, вырезали и согнули детали. Прицеп по конструкции является бескаркасным. Казалось бы, что тут делов, собрал и поехал. Но это был первый опытный образец и многое пришлось "доработать напильником". Также много делалось с нуля, так как на заводе была изготовлена только основа.</p><p> </p><p>
Изготовил новую ось со ступицами с тормозом наката.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-87517200-1391285745.jpg" data-fileid="28745" data-fileext="jpg" rel=""><img data-fileid="28745" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-87517200-1391285745_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-87517200-1391285745_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-06282500-1391285751.jpg" data-fileid="28746" data-fileext="jpg" rel=""><img data-fileid="28746" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-06282500-1391285751_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-06282500-1391285751_thumb.jpg"></a></p><p> </p><p>
Ступеньки, на которых будут размещаться канистры и заливная горловина для баков с водой.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-17913000-1391285961.jpg" data-fileid="28755" data-fileext="jpg" rel=""><img data-fileid="28755" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-17913000-1391285961_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-17913000-1391285961_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-91962200-1391285964.jpg" data-fileid="28756" data-fileext="jpg" rel=""><img data-fileid="28756" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-91962200-1391285964_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-91962200-1391285964_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-67497800-1391285969.jpg" data-fileid="28757" data-fileext="jpg" rel=""><img data-fileid="28757" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-67497800-1391285969_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-67497800-1391285969_thumb.jpg"></a></p><p> </p><p>
Установлено два бака по 70 литров. Для каждого бака защита из 6-ти миллиметрового алюминия.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-93430900-1391286069.jpg" data-fileid="28759" data-fileext="jpg" rel=""><img data-fileid="28759" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-93430900-1391286069_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-93430900-1391286069_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-29435000-1391286078.jpg" data-fileid="28762" data-fileext="jpg" rel=""><img data-fileid="28762" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-29435000-1391286078_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-29435000-1391286078_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-92454700-1391286073.jpg" data-fileid="28760" data-fileext="jpg" rel=""><img data-fileid="28760" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-92454700-1391286073_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-92454700-1391286073_thumb.jpg"></a></p><p> </p><p>
Кронштейн для маркизы с регулировкой по высоте.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-54251900-1391286169.jpg" data-fileid="28768" data-fileext="jpg" rel=""><img data-fileid="28768" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-54251900-1391286169_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-54251900-1391286169_thumb.jpg"></a></p><p> </p><p>
Ящик на дышле для канистр и газового баллона.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-24115900-1391286244.jpg" data-fileid="28770" data-fileext="jpg" rel=""><img data-fileid="28770" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-24115900-1391286244_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-24115900-1391286244_thumb.jpg"></a></p><p> </p><p>
В боковом ящике установлен насос для воды с ресивером и приборы показывающие уровень воды в баках.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-81389800-1391286346.jpg" data-fileid="28771" data-fileext="jpg" rel=""><img data-fileid="28771" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-81389800-1391286346_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-81389800-1391286346_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-27190500-1391286353.jpg" data-fileid="28772" data-fileext="jpg" rel=""><img data-fileid="28772" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-27190500-1391286353_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-27190500-1391286353_thumb.jpg"></a></p><p> </p><p>
Палатка на крыше прицепа.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-24928500-1391286459.jpg" data-fileid="28775" data-fileext="jpg" rel=""><img data-fileid="28775" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-24928500-1391286459_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-24928500-1391286459_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-83611300-1391286451.jpg" data-fileid="28773" data-fileext="jpg" rel=""><img data-fileid="28773" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-83611300-1391286451_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-83611300-1391286451_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-68615900-1391286455.jpg" data-fileid="28774" data-fileext="jpg" rel=""><img data-fileid="28774" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-68615900-1391286455_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-68615900-1391286455_thumb.jpg"></a></p><p> </p><p>
Все детали покрашены и установлены. Прицеп готов к путешествию.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-07891100-1391286596.jpg" data-fileid="28776" data-fileext="jpg" rel=""><img data-fileid="28776" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-07891100-1391286596_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-07891100-1391286596_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-22499500-1391286600.jpg" data-fileid="28777" data-fileext="jpg" rel=""><img data-fileid="28777" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-22499500-1391286600_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-22499500-1391286600_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-29814900-1391286608.jpg" data-fileid="28778" data-fileext="jpg" rel=""><img data-fileid="28778" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-29814900-1391286608_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-29814900-1391286608_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-03293700-1391286613.jpg" data-fileid="28779" data-fileext="jpg" rel=""><img data-fileid="28779" class="ipsImage ipsImage_thumbnailed" alt="post-11238-0-03293700-1391286613_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11238-0-03293700-1391286613_thumb.jpg"></a></p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа № 30</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3791</guid><pubDate>Tue, 04 Feb 2014 13:34:32 +0000</pubDate></item><item><title>&#x41A;&#x43E;&#x43D;&#x43A;&#x443;&#x440;&#x441;: &#x441;&#x43E;&#x432;&#x435;&#x442;&#x44B;, &#x440;&#x435;&#x43A;&#x43E;&#x43C;&#x435;&#x43D;&#x434;&#x430;&#x446;&#x438;&#x438;, &#x437;&#x430;&#x43C;&#x435;&#x447;&#x430;&#x43D;&#x438;&#x44F;</title><link>https://websvarka.ru/talk/topic/4016-konkurs-sovety-rekomendatsii-zamechaniya/</link><description><![CDATA[<p>Кому интересно, то готов обсудить Конкурс. Выслушаю любые рекомендации, советы и замечания на будущее. Постараюсь ответить на все вопросы, которые будут идти в рамках нормальной дискуссии. На пустые отзывы вроде "все хорошо (плохо)", "конкурс плохой (хороший)" и т.п. — не реагирую. Интересны предложения как по Правилам, так и по спонсорству. Какие должны быть призы на аналогичных конкурсах? Сколько? Как и кем распределяются? Номинации? Сколько? Как выбирать победителя? Как проверять присланные работы? Когда проводить конкурс? И т.д.</p><p> </p><p>Для создания общей картины прикрепляю несколько опросов (голосование открытое). По мере необходимости добавлю еще опрос в тему (пишите предложения).</p><p> </p><p>Дополнительная информация по конкурсу.</p><ul><li>Всего было прислано на конкурс ~105 работ. Работы падали как сразу в премодерацию в конкурсный раздел, так мне на электронную почту и личные сообщения на форуме.</li><li>До участия в конкурсе было допущено 75 работ.</li><li>В итоговом голосовании приняли участие 226 пользователей форума (при планировании конкурса я рассчитывал на 100).</li><li>226 пользователей раздали 1430 голосов.</li><li>В "среднем по больнице" каждый пользователь выбирал по 6 работ из 75.</li></ul>]]></description><guid isPermaLink="false">4016</guid><pubDate>Wed, 05 Mar 2014 17:42:41 +0000</pubDate></item><item><title>&#x41F;&#x435;&#x440;&#x435;&#x43D;&#x43E;&#x441;&#x43D;&#x43E;&#x439; &#x448;&#x43B;&#x438;&#x444;&#x43E;&#x432;&#x430;&#x43B;&#x44C;&#x43D;&#x44B;&#x439; &#x441;&#x442;&#x430;&#x43D;&#x43E;&#x43A;</title><link>https://websvarka.ru/talk/topic/3820-perenosnoy-shlifovalnyy-stanok/</link><description><![CDATA[
<p>У восстанавливаемого в моей мастерской «из руин» токарно-винторезного станка 16К20 большой износ направляющих станины — более 0,4 мм. Направляющие можно отшлифовать в заводских условиях (необходима полная разборка станка, да и дорого) или отшабрить вручную. Но второй вариант вообще проблематичен, так как направляющие на этом станке закалены, т.е. термообработаны до высокой твердости металла.</p><p> </p><p>
Для выхода из сложившейся ситуации был разработан и изготовлен переносной шлифовальный станок (здесь и далее ПШС) для шлифовки призматических и плоских направляющих станин токарных станков типа 1А616, 1К62, 16К20 и др.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3573-0-18444500-1391587386.jpg" data-fileid="29071" data-fileext="jpg" rel=""><img data-fileid="29071" class="ipsImage ipsImage_thumbnailed" alt="post-3573-0-18444500-1391587386_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3573-0-18444500-1391587386_thumb.jpg"></a></p><p> </p><p>
Состоит из следующих основных узлов: стойки, выдвижной пиноли и шлифовальной головки. ПШС позволяет, не демонтируя и не полностью разбирая ремонтируемый станок, осуществить шлифовку изношенных направляющих в условиях любого гаража и мастерской. Базируется ПШС по направляющим задней балки, перемещается с помощью ручной тросовой лебедки, снабжен контргрузами. Привод шлифовальной головки имеет мощность 0,42 кВт, 3000 об/мин., 3 ф. Для охлаждения шлифовального камня и удаления отработанного абразива из зоны шлифовки имеется система подачи смазочно-охлаждающей жидкости (СОЖ) с помощью штатного насоса ремонтируемого станка.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3573-0-53907300-1391587369.jpg" data-fileid="29070" data-fileext="jpg" rel=""><img data-fileid="29070" class="ipsImage ipsImage_thumbnailed" alt="post-3573-0-53907300-1391587369_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3573-0-53907300-1391587369_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3573-0-19207600-1391587427.jpg" data-fileid="29072" data-fileext="jpg" rel=""><img data-fileid="29072" class="ipsImage ipsImage_thumbnailed" alt="post-3573-0-19207600-1391587427_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3573-0-19207600-1391587427_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3573-0-84381200-1391587520.jpg" data-fileid="29073" data-fileext="jpg" rel=""><img data-fileid="29073" class="ipsImage ipsImage_thumbnailed" alt="post-3573-0-84381200-1391587520_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-3573-0-84381200-1391587520_thumb.jpg"></a></p><p> </p><p>
Все детали изготавливались на моём токарном станке 1А616К, сварка велась полуавтоматом. Стойка куплена в пункте приёма металлолома, пиноль изготовлена из задней бабки станка 1А616, купленного на форуме у чипмейкеров.</p><p> </p><p>
Есть небольшие видеоматериалы, наглядно иллюстрирующие работу ПШС.</p><p>
<a href="http://www.youtube.com/watch?v=3muDDBxWdgY" rel="external nofollow">http://www.youtube.com/watch?v=3muDDBxWdgY</a></p><p>
<a href="http://www.youtube.com/watch?v=f8evpdGsrwE" rel="external nofollow">http://www.youtube.com/watch?v=f8evpdGsrwE</a></p><p> </p><p>
Всем удачи в конкурсе! Пусть победит лучший и достойнейший!</p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа № 35</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3820</guid><pubDate>Thu, 06 Feb 2014 14:54:49 +0000</pubDate></item><item><title>&#x41A;&#x43E;&#x43F;&#x442;&#x438;&#x43B;&#x43A;&#x430;</title><link>https://websvarka.ru/talk/topic/3652-koptilka/</link><description><![CDATA[
<p><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-57954200-1389970787.jpg" data-fileid="27353" data-fileext="jpg" rel=""><img data-fileid="27353" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-57954200-1389970787_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-57954200-1389970787_thumb.jpg"></a></p><p> </p><p>
Чисто случайно наткнулся на эту идею в интернете и, не долго думая, воплотил в жизнь. Вариантов реализации дыма по этому принципу несколько. Делал, собственно, одну версию, но компрессор для неё оказался слабоват, надо помощнее — работоспособность показана при помощи резака (кислород "подогревающий" слегка приоткрыл и пошло). Потерпев временное фиаско на первом этапе, быстро реализовал второй вариант, изменив схему, и конструкция заработала. В дальнейшем все огрехи доработаются, но суть схемы, думаю, ясна. Преимущества в том, что копчение получается холодным без глобальных конструкций. Достаточно, образно говоря, картонной коробки — ради прикола пачку от электродов водрузил (для перестраховки можно удлинить/нарастить трубу немного). Процесс не требует постоянного контроля, ну и малобюджетный. Для меня этот вариант в диковинку, но заинтересовал по-серьёзному, думаю, что не только мне это будет интересно. Хотел в 1000 мелочей запостить, но потом решил пополнить конкурсную тему, а то начало "битвы" неактивное. Куча снимков не требует пояснений — принцип, проще пареной репы, а видео дополнит картину. Второй вариант не "расписывал", времени не было, но на видео я детали показал.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-08499400-1389970657.jpg" data-fileid="27339" data-fileext="jpg" rel=""><img data-fileid="27339" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-08499400-1389970657_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-08499400-1389970657_thumb.jpg"></a> <a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-07104800-1389970664.jpg" data-fileid="27340" data-fileext="jpg" rel=""><img data-fileid="27340" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-07104800-1389970664_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-07104800-1389970664_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-11784900-1389970671.jpg" data-fileid="27341" data-fileext="jpg" rel=""><img data-fileid="27341" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-11784900-1389970671_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-11784900-1389970671_thumb.jpg"></a> <a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-78442900-1389970679.jpg" data-fileid="27342" data-fileext="jpg" rel=""><img data-fileid="27342" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-78442900-1389970679_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-78442900-1389970679_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-06640100-1389970690.jpg" data-fileid="27343" data-fileext="jpg" rel=""><img data-fileid="27343" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-06640100-1389970690_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-06640100-1389970690_thumb.jpg"></a> <a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-41054700-1389970704.jpg" data-fileid="27344" data-fileext="jpg" rel=""><img data-fileid="27344" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-41054700-1389970704_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-41054700-1389970704_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-16476400-1389970712.jpg" data-fileid="27345" data-fileext="jpg" rel=""><img data-fileid="27345" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-16476400-1389970712_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-16476400-1389970712_thumb.jpg"></a> <a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-78418100-1389970719.jpg" data-fileid="27346" data-fileext="jpg" rel=""><img data-fileid="27346" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-78418100-1389970719_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-78418100-1389970719_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-94439000-1389970730.jpg" data-fileid="27347" data-fileext="jpg" rel=""><img data-fileid="27347" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-94439000-1389970730_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-94439000-1389970730_thumb.jpg"></a> <a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-98350900-1389970741.jpg" data-fileid="27348" data-fileext="jpg" rel=""><img data-fileid="27348" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-98350900-1389970741_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-98350900-1389970741_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-33526100-1389970753.jpg" data-fileid="27349" data-fileext="jpg" rel=""><img data-fileid="27349" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-33526100-1389970753_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-33526100-1389970753_thumb.jpg"></a> <a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-89457100-1389970761.jpg" data-fileid="27350" data-fileext="jpg" rel=""><img data-fileid="27350" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-89457100-1389970761_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-89457100-1389970761_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-40712100-1389970771.jpg" data-fileid="27351" data-fileext="jpg" rel=""><img data-fileid="27351" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-40712100-1389970771_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-40712100-1389970771_thumb.jpg"></a> <a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-24800900-1389970779.jpg" data-fileid="27352" data-fileext="jpg" rel=""><img data-fileid="27352" class="ipsImage ipsImage_thumbnailed" alt="post-699-0-24800900-1389970779_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-699-0-24800900-1389970779_thumb.jpg"></a></p><p> </p><p>
Можно всё сделать на сварке, дабы упростить конструкцию, но так как это опытный вариант и всё делается методом проб и ошибок, с регулировкой и вымерением зазоров расстояний, то пока так. Хотя если подача воздуха достаточная, то "протянет" любой зазор. Проблема возникла с опилками, у нас в цеху только металлические, пришлось к мебельщикам идти. Запах "копчения" был специфический.</p><p> </p><p>
<a href="http://www.youtube.com/watch?v=eXvb22tDLrk" rel="external nofollow">http://www.youtube.com/watch?v=eXvb22tDLrk</a></p><p>
<a href="http://www.youtube.com/watch?v=l6TxZImDN4I" rel="external nofollow">http://www.youtube.com/watch?v=l6TxZImDN4I</a></p><p> </p><p>
Чуть не забыл <img alt=":pardon:" src="https://websvarka.ru/talk/uploads/emoticons/default_pardon.gif"> <img alt=":crazy:" src="https://websvarka.ru/talk/uploads/emoticons/default_crazy.gif">. Заводим сей агрегат зажигалкой, через отверстия снизу, предварительно включив аквариумный компрессор (я за него забыл упомянуть, у меня он на 300 л/ч, повторюсь, маловат). Вставляем дышло в тару с продуктом и через опытным путём подобранное время, наслаждаемся копчёностями. Думаю, что и на балконе можно реализовать небольшое производство.</p><p> </p><p>
Ссылка на первоисточник (ну а там и дальше по ссылкам ) <a href="http://www.youtube.com/watch?v=AzP76bNxt4o" rel="external nofollow">Smokai Smoke Generator</a></p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа №3</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3652</guid><pubDate>Fri, 17 Jan 2014 15:13:14 +0000</pubDate></item><item><title>&#x410;&#x43B;&#x44E;&#x43C;&#x438;&#x43D;&#x438;&#x435;&#x432;&#x430;&#x44F; &#x43B;&#x43E;&#x434;&#x43A;&#x430;</title><link>https://websvarka.ru/talk/topic/3893-alyuminievaya-lodka/</link><description><![CDATA[
<p>Зовут меня Виктор. Живу в пригороде г. Воронежа. Занимаюсь строительством алюминиевых лодок 13 лет. Первую лодку построил в 2001 году, когда жил на Камчатке. Сейчас строю не большие бюджетные лодки на заказ.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11342-0-10531000-1392391243.jpg" data-fileid="30102" data-fileext="jpg" rel=""><img data-fileid="30102" class="ipsImage ipsImage_thumbnailed" alt="post-11342-0-10531000-1392391243_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11342-0-10531000-1392391243_thumb.jpg"></a></p><p> </p><p>
Использую материал АМГ5М, листы толщиной 2мм. Для предания жёсткости корпуса лодки делаю зиги по бортам и на днище судна. Корпус лодки сварной-клёпаный. Применяю клёпку для установки шпангоутов, чтобы было меньше деформации. На изготовление одной лодки длиной 3.85 м уходит одна неделя.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11342-0-92126900-1392391346.jpg" data-fileid="30103" data-fileext="jpg" rel=""><img data-fileid="30103" class="ipsImage ipsImage_thumbnailed" alt="post-11342-0-92126900-1392391346_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11342-0-92126900-1392391346_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11342-0-68070200-1392391458.jpg" data-fileid="30104" data-fileext="jpg" rel=""><img data-fileid="30104" class="ipsImage ipsImage_thumbnailed" alt="post-11342-0-68070200-1392391458_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11342-0-68070200-1392391458_thumb.jpg"></a></p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа № 57</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3893</guid><pubDate>Sun, 16 Feb 2014 12:23:22 +0000</pubDate></item><item><title>&#x41A;&#x43E;&#x43C;&#x43F;&#x430;&#x43A;&#x442;&#x43D;&#x430;&#x44F; &#x43F;&#x435;&#x447;&#x44C; &#x43D;&#x430; &#x43E;&#x442;&#x440;&#x430;&#x431;&#x43E;&#x442;&#x430;&#x43D;&#x43D;&#x43E;&#x43C; &#x43C;&#x430;&#x441;&#x43B;&#x435;</title><link>https://websvarka.ru/talk/topic/3749-kompaktnaya-pech-na-otrabotannom-masle/</link><description><![CDATA[
<p>Привет всем! Меня зовут Сергей Клянчин. Я работаю на автозаводе УАЗ инженером. В свое время мне понадобилась компактная печь для обогрева своей маленькой мастерской. За тип топлива взял отработанное масло. Конструкций малого размера не нашел, пришлось мудрить самому, изучив конструкции промышленных обогревателей. Пришлось несколько раз переделывать и менять конструкцию. Работал вечерами после работы.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-612-0-19440600-1390911726.jpg" data-fileid="28272" data-fileext="jpg" rel=""><img data-fileid="28272" class="ipsImage ipsImage_thumbnailed" alt="post-612-0-19440600-1390911726_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-612-0-19440600-1390911726_thumb.jpg"></a></p><p> </p><p>
Корпус печи изготовлен из металла толщиной 3мм, усилен для жесткости ребрами. Горелка и горизонтальная часть теплообменника изготовлена из толстостенной трубы 106 мм. Принцип печи - капельница с предварительным подогревом масла и принудительным наддувом воздуха в камеру сгорания. Нижняя часть камеры легкосъемная для чистки. Имеются также два мотора - вентилятора продувки воздуха помещения через теплообменник для более быстрого прогрева. Сверху на трубе в дальнейшем был установлен съемный бачок для нагрева воды (руки помыть после работы). Вес печи примерно 40 кг, расход масла 0,5-1,7 литра в час. Отдача в районе 5-15 квт (субъективная оценка). Температура нагретого воздуха из печи 80-130 градусов (в зависимости от настройки мощности). Печь не пожароопасна при попадания воды и антифриза в масло. Был заменен краник слива отстоя из масляного бака на более производительный. На части фото присутствует еще старый вариант. Далее немного фото и видео с описанием.</p><p> </p><p>
Размеры</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-612-0-09575000-1390911694.jpg" data-fileid="28271" data-fileext="jpg" rel=""><img data-fileid="28271" class="ipsImage ipsImage_thumbnailed" alt="post-612-0-09575000-1390911694_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-612-0-09575000-1390911694_thumb.jpg"></a></p><p> </p><p>
Изготовление масляного бака</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-14391200-1391069661.jpg" data-fileid="28424" data-fileext="jpg" rel=""><img data-fileid="28424" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-14391200-1391069661_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-14391200-1391069661_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-55896100-1391069660.jpg" data-fileid="28423" data-fileext="jpg" rel=""><img data-fileid="28423" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-55896100-1391069660_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-55896100-1391069660_thumb.jpg"></a></p><p> </p><p>
Изготовление обменника</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-86179500-1391069707.jpg" data-fileid="28425" data-fileext="jpg" rel=""><img data-fileid="28425" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-86179500-1391069707_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-86179500-1391069707_thumb.jpg"></a></p><p> </p><p>
Этап сборки</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-41929700-1391069734.jpg" data-fileid="28426" data-fileext="jpg" rel=""><img data-fileid="28426" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-41929700-1391069734_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-41929700-1391069734_thumb.jpg"></a></p><p> </p><p>
Бак нагрева масла</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-07940000-1391069805.jpg" data-fileid="28427" data-fileext="jpg" rel=""><img data-fileid="28427" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-07940000-1391069805_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-07940000-1391069805_thumb.jpg"></a></p><p> </p><p>
Вентиляторы продувки</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-26251000-1391069841.jpg" data-fileid="28428" data-fileext="jpg" rel=""><img data-fileid="28428" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-26251000-1391069841_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-26251000-1391069841_thumb.jpg"></a></p><p> </p><p>
Камера сгорания</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-44368200-1391069869.jpg" data-fileid="28429" data-fileext="jpg" rel=""><img data-fileid="28429" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-44368200-1391069869_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-44368200-1391069869_thumb.jpg"></a></p><p> </p><p>
Капельница</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-02481700-1391069901.jpg" data-fileid="28430" data-fileext="jpg" rel=""><img data-fileid="28430" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-02481700-1391069901_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-02481700-1391069901_thumb.jpg"></a></p><p> </p><p>
Крыльчатка нагнетания воздуха</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-53115900-1391069943.jpg" data-fileid="28431" data-fileext="jpg" rel=""><img data-fileid="28431" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-53115900-1391069943_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-53115900-1391069943_thumb.jpg"></a></p><p> </p><p>
Общие виды</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-75674800-1391069998.jpg" data-fileid="28432" data-fileext="jpg" rel=""><img data-fileid="28432" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-75674800-1391069998_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-75674800-1391069998_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-13377600-1391070004.jpg" data-fileid="28433" data-fileext="jpg" rel=""><img data-fileid="28433" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-13377600-1391070004_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-13377600-1391070004_thumb.jpg"></a></p><p> </p><p>
Поджиг печи</p><p>
<a href="http://www.youtube.com/watch?v=4DcIqTsIeA0" rel="external nofollow">http://www.youtube.com/watch?v=4DcIqTsIeA0</a></p><p> </p><p>
Печь вышла на максимальный режим</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-53226800-1391070072.jpg" data-fileid="28434" data-fileext="jpg" rel=""><img data-fileid="28434" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-53226800-1391070072_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-53226800-1391070072_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-05515400-1391070073.jpg" data-fileid="28435" data-fileext="jpg" rel=""><img data-fileid="28435" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-05515400-1391070073_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-05515400-1391070073_thumb.jpg"></a></p><p> </p><p>
Спасибо за внимание</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-612-0-52606900-1390911812.jpg" data-fileid="28274" data-fileext="jpg" rel=""><img data-fileid="28274" class="ipsImage ipsImage_thumbnailed" alt="post-612-0-52606900-1390911812_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-612-0-52606900-1390911812_thumb.jpg"></a></p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа № 22</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3749</guid><pubDate>Thu, 30 Jan 2014 11:44:51 +0000</pubDate></item><item><title>&#x411;&#x412;&#x41E; &#x438;&#x43B;&#x438; &#x432;&#x43E;&#x434;&#x44F;&#x43D;&#x43E;&#x435; &#x43E;&#x445;&#x43B;&#x430;&#x436;&#x434;&#x435;&#x43D;&#x438;&#x435;</title><link>https://websvarka.ru/talk/topic/3911-bvo-ili-vodyanoe-ohlazhdenie/</link><description><![CDATA[
<p>Доброго здравия! Решил выставить свою работу на конкурс. После покупки аппарата задумался об охлаждении горелки. Просмотр предложений на фирмах не соответствовал моим запросам (БВО нужен горизонтального типа, возможность поставить на него сварочный аппарат, вес 40 кг). Приблизительные размеры были, что требовалось для изготовления присматривал. Поиск подходящих комплектующих затянулся... Через несколько дней всё приобретено. Сварить каркас корпуса из профильной трубы не составило большого труда (обрезков трубы достаточно). Придумать крепление радиатора и вентиляторов, найти место установки насоса. Подходящий радиатор нашёл случайно, по размерам подходил в самый раз. После установки вентиляторов, радиатора и насоса пришло время изготовления бака. Прежде чем начал варить бак, подумал о направлении потока воздуха из радиатора. Надо направить поток на боковые стенки. Из этих соображений принял решение — корпус бака должен быть с радиальным скруглением. Сварил бак, установил на место. Подсоединил трубопроводы. С боковыми стенками корпуса пришлось повозиться. Изготовил простой пуансон для гибки профильной решетки. Разметка, пропил пазов, гибка, после сборки обработка. Пришло время для электической части: паяльник, зажимные клещи и клемы. Собрал и запустил. Работает.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-9285-0-87755200-1392569465.jpg" data-fileid="30417" data-fileext="jpg" rel=""><img data-fileid="30417" class="ipsImage ipsImage_thumbnailed" alt="post-9285-0-87755200-1392569465_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-9285-0-87755200-1392569465_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-9285-0-79983000-1392569497.jpg" data-fileid="30418" data-fileext="jpg" rel=""><img data-fileid="30418" class="ipsImage ipsImage_thumbnailed" alt="post-9285-0-79983000-1392569497_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-9285-0-79983000-1392569497_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-9285-0-43758800-1392569532.jpg" data-fileid="30420" data-fileext="jpg" rel=""><img data-fileid="30420" class="ipsImage ipsImage_thumbnailed" alt="post-9285-0-43758800-1392569532_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-9285-0-43758800-1392569532_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-9285-0-37218700-1392569614.jpg" data-fileid="30421" data-fileext="jpg" rel=""><img data-fileid="30421" class="ipsImage ipsImage_thumbnailed" alt="post-9285-0-37218700-1392569614_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-9285-0-37218700-1392569614_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-9285-0-99888200-1392569682.jpg" data-fileid="30423" data-fileext="jpg" rel=""><img data-fileid="30423" class="ipsImage ipsImage_thumbnailed" alt="post-9285-0-99888200-1392569682_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-9285-0-99888200-1392569682_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-9285-0-63482200-1392569747.jpg" data-fileid="30425" data-fileext="jpg" rel=""><img data-fileid="30425" class="ipsImage ipsImage_thumbnailed" alt="post-9285-0-63482200-1392569747_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-9285-0-63482200-1392569747_thumb.jpg"></a></p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа № 63</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3911</guid><pubDate>Mon, 17 Feb 2014 13:43:27 +0000</pubDate></item><item><title>&#x41C;&#x443;&#x445;&#x430; &#x426;&#x43E;&#x43A;&#x43E;&#x442;&#x443;&#x445;&#x430;</title><link>https://websvarka.ru/talk/topic/3919-muha-tsokotuha/</link><description><![CDATA[
<p>Выставляю на Ваш суд «Муху Цокотуху» из нержавеющей стали - мой первый опыт в художественной сварке!</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-37657300-1392608226.jpg" data-fileid="30473" data-fileext="jpg" rel=""><img data-fileid="30473" class="ipsImage ipsImage_thumbnailed" alt="post-11360-0-37657300-1392608226_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-37657300-1392608226_thumb.jpg"></a></p><p> </p><p>
Для ее изготовления я использовала нержавеющую сталь 1 мм и присадочную проволоку 1,6 мм с последующим обжигом (для цвета) бытовой пропановой горелкой. «Пяточёк» не моих рук дело — произведение Гознака <img alt=":)" src="https://websvarka.ru/talk/uploads/emoticons/default_smile.png"></p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-62189200-1392608251.jpg" data-fileid="30474" data-fileext="jpg" rel=""><img data-fileid="30474" class="ipsImage ipsImage_thumbnailed" alt="post-11360-0-62189200-1392608251_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-62189200-1392608251_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-50182800-1392608270.jpg" data-fileid="30475" data-fileext="jpg" rel=""><img data-fileid="30475" class="ipsImage ipsImage_thumbnailed" alt="post-11360-0-50182800-1392608270_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-50182800-1392608270_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-37416500-1392608297.jpg" data-fileid="30476" data-fileext="jpg" rel=""><img data-fileid="30476" class="ipsImage ipsImage_thumbnailed" alt="post-11360-0-37416500-1392608297_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-37416500-1392608297_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-73928200-1392608315.jpg" data-fileid="30477" data-fileext="jpg" rel=""><img data-fileid="30477" class="ipsImage ipsImage_thumbnailed" alt="post-11360-0-73928200-1392608315_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-73928200-1392608315_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-46627000-1392608342.jpg" data-fileid="30478" data-fileext="jpg" rel=""><img data-fileid="30478" class="ipsImage ipsImage_thumbnailed" alt="post-11360-0-46627000-1392608342_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-46627000-1392608342_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-85514000-1392608362.jpg" data-fileid="30479" data-fileext="jpg" rel=""><img data-fileid="30479" class="ipsImage ipsImage_thumbnailed" alt="post-11360-0-85514000-1392608362_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-85514000-1392608362_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-93841800-1392608415.jpg" data-fileid="30481" data-fileext="jpg" rel=""><img data-fileid="30481" class="ipsImage ipsImage_thumbnailed" alt="post-11360-0-93841800-1392608415_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11360-0-93841800-1392608415_thumb.jpg"></a></p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа № 65</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3919</guid><pubDate>Tue, 18 Feb 2014 13:16:53 +0000</pubDate></item><item><title>&#x41D;&#x430;&#x431;&#x43E;&#x440; &#x440;&#x44E;&#x43C;&#x43E;&#x43A; &#xAB;&#x41D;&#x430; &#x441;&#x43E;&#x43C;&#x430;&#xBB;</title><link>https://websvarka.ru/talk/topic/3740-nabor-ryumok-%C2%ABna-soma%C2%BB/</link><description><![CDATA[
<p><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-25899600-1390896473.jpg" data-fileid="28245" data-fileext="jpg" rel=""><img data-fileid="28245" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-25899600-1390896473_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-25899600-1390896473_thumb.jpg"></a><br> <br>Набор из 6 рюмок (ёмкость 35 мл), длина "лодки" - 350 мм. Сварка п/автоматом в среде углекислого газа.<br> <br><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-46192300-1390896686.jpg" data-fileid="28246" data-fileext="jpg" rel=""><img data-fileid="28246" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-46192300-1390896686_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-46192300-1390896686_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-07774400-1390896687.jpg" data-fileid="28247" data-fileext="jpg" rel=""><img data-fileid="28247" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-07774400-1390896687_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-07774400-1390896687_thumb.jpg"></a></p><p><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-73517400-1390896687.jpg" data-fileid="28248" data-fileext="jpg" rel=""><img data-fileid="28248" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-73517400-1390896687_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-73517400-1390896687_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-93079000-1390896688.jpg" data-fileid="28250" data-fileext="jpg" rel=""><img data-fileid="28250" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-93079000-1390896688_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-93079000-1390896688_thumb.jpg"></a></p><p><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-25881100-1390896688.jpg" data-fileid="28249" data-fileext="jpg" rel=""><img data-fileid="28249" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-25881100-1390896688_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-25881100-1390896688_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-23895900-1390896690.jpg" data-fileid="28251" data-fileext="jpg" rel=""><img data-fileid="28251" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-23895900-1390896690_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-23895900-1390896690_thumb.jpg"></a></p><p><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-30226100-1390896691.jpg" data-fileid="28252" data-fileext="jpg" rel=""><img data-fileid="28252" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-30226100-1390896691_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-30226100-1390896691_thumb.jpg"></a></p><p> </p><div><hr></div><div><strong>Конкурсная работа № 19</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></div><div> </div><div><strong>Спонсоры Конкурса</strong></div><div><a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</div><div><a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></div><div> </div><div><a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</div><div><a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></div><div> </div><div><a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</div><div><a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></div>
]]></description><guid isPermaLink="false">3740</guid><pubDate>Tue, 28 Jan 2014 08:15:48 +0000</pubDate></item><item><title>&#x41C;&#x430;&#x43D;&#x433;&#x430;&#x43B; &#xAB;&#x41E;&#x43B;&#x435;&#x43D;&#x44C;&#xBB;</title><link>https://websvarka.ru/talk/topic/3815-mangal-%C2%ABolen%C2%BB/</link><description><![CDATA[
<p><span style="font-size:14px;">Здравствуйте. Меня зовут Юрий, мне 22 года. Учусь в Российской </span>академии живописи, ваяния и зодчества Ильи Глазунова<span style="font-size:14px;"> на втором курсе, по специальности декоративно-прикладное искусство. </span>Представляю вашему вниманию свою работу. Её я сделал специально для конкурса.</p><p>
 </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-73714000-1391535581.jpg" data-fileid="29025" data-fileext="jpg" rel=""><img data-fileid="29025" class="ipsImage ipsImage_thumbnailed" alt="post-7618-0-73714000-1391535581_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-73714000-1391535581_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-14008200-1391535604.jpg" data-fileid="29026" data-fileext="jpg" rel=""><img data-fileid="29026" class="ipsImage ipsImage_thumbnailed" alt="post-7618-0-14008200-1391535604_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-14008200-1391535604_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-40729000-1391535655.jpg" data-fileid="29028" data-fileext="jpg" rel=""><img data-fileid="29028" class="ipsImage ipsImage_thumbnailed" alt="post-7618-0-40729000-1391535655_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-40729000-1391535655_thumb.jpg"></a></p><p>
 </p><p>
Для изготовления я использовал материал: газовый баллон от автомобиля 60 литров, сталь листовая 2 мм и 8 мм. Техника: выколотка, ковка, сварка (полуавтомат). Первым делом я вылепил примерный эскиз из пластилина небольшого размера. Приготовил выкройки для изготовления ног, шеи, головы. Дальше при помощи электро-ножниц выстриг выкройки. Ноги состоят из двух частей, шея из четырех, голова из четырех. Далее при помощи молотка и пенька выколачивал нужный мне объем заготовок. Собрал все части и монтировал их к баллону.</p><p>
 </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-49673900-1391537490.jpg" data-fileid="29030" data-fileext="jpg" rel=""><img data-fileid="29030" class="ipsImage ipsImage_thumbnailed" alt="post-7618-0-49673900-1391537490_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-49673900-1391537490_thumb.jpg"></a> <a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-48948100-1391537504.jpg" data-fileid="29031" data-fileext="jpg" rel=""><img data-fileid="29031" class="ipsImage ipsImage_thumbnailed" alt="post-7618-0-48948100-1391537504_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-48948100-1391537504_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-07367600-1391537515.jpg" data-fileid="29033" data-fileext="jpg" rel=""><img data-fileid="29033" class="ipsImage ipsImage_thumbnailed" alt="post-7618-0-07367600-1391537515_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-07367600-1391537515_thumb.jpg"></a></p><p>
 </p><p>
Чтобы обрезки не пропадали, применил их для имитации шерсти. Отковал уши из 8 мм стали путем нагревания резаком. Таким же способом рога.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-14420000-1391537511.jpg" data-fileid="29032" data-fileext="jpg" rel=""><img data-fileid="29032" class="ipsImage ipsImage_thumbnailed" alt="post-7618-0-14420000-1391537511_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-14420000-1391537511_thumb.jpg"></a> </p><p>
 </p><p>
Из проволоки 5 мм отковал узор на крышке мангала. Раз это мангал и он будет использоваться, решил поэкспериментировать — покрыл растительным маслом и нагрел газовой горелкой, получился соломенный коричневый цвет.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-58833300-1391535559.jpg" data-fileid="29024" data-fileext="jpg" rel=""><img data-fileid="29024" class="ipsImage ipsImage_thumbnailed" alt="post-7618-0-58833300-1391535559_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-7618-0-58833300-1391535559_thumb.jpg"></a></p><p>
 </p><p>
А если начнет покрываться ржавчиной в ходе использования, не перестанет быть эстетичным. Я на это надеюсь. Изготовление мангала заняло 2 недели.</p><p>
 </p><p>
Спасибо за внимание. Пишите с удовольствием отвечу.</p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа № 36</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3815</guid><pubDate>Fri, 07 Feb 2014 10:00:21 +0000</pubDate></item><item><title>&#x411;&#x435;&#x442;&#x43E;&#x43D;&#x43E;&#x43C;&#x435;&#x448;&#x430;&#x43B;&#x43A;&#x430;</title><link>https://websvarka.ru/talk/topic/3841-betonomeshalka/</link><description><![CDATA[
<p>Здравствуйте. Узнав о конкурсе, решил изготовить бетономешалку. Давно собирался, да и строительство на весну намечается (расширение гаража). В общем конкурс — это хорошая мотивация что-то сделать своими руками.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-14881400-1391779854.jpg" data-fileid="29348" data-fileext="jpg" rel=""><img data-fileid="29348" class="ipsImage ipsImage_thumbnailed" alt="post-177-0-14881400-1391779854_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-14881400-1391779854_thumb.jpg"></a></p><p> </p><p>
Была бочка 200 литров, двигатель от советской круглой стиральной машины, чуть разного металла, авто диск, ступица и желание. Установлен таймер от той же стиралки, тумблер ручной и авто режим работы. Скорость вращения барабана где-то 35-40 об. Я не претендую на оригинальность, кое-что почерпнул из сети.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-88364700-1391779536.jpg" data-fileid="29341" data-fileext="jpg" rel=""><img data-fileid="29341" class="ipsImage ipsImage_thumbnailed" alt="post-177-0-88364700-1391779536_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-88364700-1391779536_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-56282300-1391779609.jpg" data-fileid="29342" data-fileext="jpg" rel=""><img data-fileid="29342" class="ipsImage ipsImage_thumbnailed" alt="post-177-0-56282300-1391779609_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-56282300-1391779609_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-95552700-1391779633.jpg" data-fileid="29343" data-fileext="jpg" rel=""><img data-fileid="29343" class="ipsImage ipsImage_thumbnailed" alt="post-177-0-95552700-1391779633_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-95552700-1391779633_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-87202500-1391779677.jpg" data-fileid="29344" data-fileext="jpg" rel=""><img data-fileid="29344" class="ipsImage ipsImage_thumbnailed" alt="post-177-0-87202500-1391779677_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-87202500-1391779677_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-61392400-1391779727.jpg" data-fileid="29345" data-fileext="jpg" rel=""><img data-fileid="29345" class="ipsImage ipsImage_thumbnailed" alt="post-177-0-61392400-1391779727_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-61392400-1391779727_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-85422600-1391779779.jpg" data-fileid="29346" data-fileext="jpg" rel=""><img data-fileid="29346" class="ipsImage ipsImage_thumbnailed" alt="post-177-0-85422600-1391779779_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-85422600-1391779779_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-12620500-1391779819.jpg" data-fileid="29347" data-fileext="jpg" rel=""><img data-fileid="29347" class="ipsImage ipsImage_thumbnailed" alt="post-177-0-12620500-1391779819_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-177-0-12620500-1391779819_thumb.jpg"></a></p><p> </p><p>
Буду рад участию в конкурсе. С ув.Дмитрий.</p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа № 41</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3841</guid><pubDate>Sat, 08 Feb 2014 17:43:23 +0000</pubDate></item><item><title>&#x423;&#x43A;&#x440;&#x430;&#x448;&#x435;&#x43D;&#x438;&#x44F; &#x438;&#x437; &#x442;&#x438;&#x442;&#x430;&#x43D;&#x430;</title><link>https://websvarka.ru/talk/topic/3933-ukrasheniya-iz-titana/</link><description><![CDATA[
<p>Здравствуйте, дорогие дугопоклонники! Представляю на Ваш справедливый суд некоторые мои работы. Выполнены они из титановой проволоки методом наплавления аргонодуговой сваркой, а также раскраской путём теплового воздействия сварочной дугой. В этих работах я сознательно придерживался принципа «как пойдёт». Титан — материал норовистый и даже самому опытному мастеру вносит свои коррективы. Я старался подражать природным и абстрактным формам.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-66414600-1392759130.jpg" data-fileid="30685" data-fileext="jpg" rel=""><img data-fileid="30685" class="ipsImage ipsImage_thumbnailed" alt="post-11344-0-66414600-1392759130_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-66414600-1392759130_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-09510100-1392759161.jpg" data-fileid="30686" data-fileext="jpg" rel=""><img data-fileid="30686" class="ipsImage ipsImage_thumbnailed" alt="post-11344-0-09510100-1392759161_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-09510100-1392759161_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-34831600-1392759236.jpg" data-fileid="30689" data-fileext="jpg" rel=""><img data-fileid="30689" class="ipsImage ipsImage_thumbnailed" alt="post-11344-0-34831600-1392759236_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-34831600-1392759236_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-16083000-1392759259.jpg" data-fileid="30690" data-fileext="jpg" rel=""><img data-fileid="30690" class="ipsImage ipsImage_thumbnailed" alt="post-11344-0-16083000-1392759259_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-16083000-1392759259_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-78458900-1392759285.jpg" data-fileid="30691" data-fileext="jpg" rel=""><img data-fileid="30691" class="ipsImage ipsImage_thumbnailed" alt="post-11344-0-78458900-1392759285_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-78458900-1392759285_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-84987100-1392759310.jpg" data-fileid="30692" data-fileext="jpg" rel=""><img data-fileid="30692" class="ipsImage ipsImage_thumbnailed" alt="post-11344-0-84987100-1392759310_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-84987100-1392759310_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-62891100-1392759334.jpg" data-fileid="30693" data-fileext="jpg" rel=""><img data-fileid="30693" class="ipsImage ipsImage_thumbnailed" alt="post-11344-0-62891100-1392759334_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-62891100-1392759334_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-93746500-1392759400.jpg" data-fileid="30695" data-fileext="jpg" rel=""><img data-fileid="30695" class="ipsImage ipsImage_thumbnailed" alt="post-11344-0-93746500-1392759400_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-93746500-1392759400_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-55353400-1392759380.jpg" data-fileid="30694" data-fileext="jpg" rel=""><img data-fileid="30694" class="ipsImage ipsImage_thumbnailed" alt="post-11344-0-55353400-1392759380_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-55353400-1392759380_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-10272400-1392759191.jpg" data-fileid="30687" data-fileext="jpg" rel=""><img data-fileid="30687" class="ipsImage ipsImage_thumbnailed" alt="post-11344-0-10272400-1392759191_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-11344-0-10272400-1392759191_thumb.jpg"></a></p><p>
 </p><p>
</p><hr><p>
<strong>Конкурсная работа № 71</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3933</guid><pubDate>Wed, 19 Feb 2014 10:19:04 +0000</pubDate></item><item><title>&#x414;&#x440;&#x430;&#x43A;&#x43E;&#x43D;&#x44B;</title><link>https://websvarka.ru/talk/topic/3734-drakony/</link><description><![CDATA[
<p>Меня зовут МАГ — это мои инициалы, хотя друзья уверены, что я еще и волшебник. Но я не волшебник, я только учусь. Я сам не являюсь сварщиком «профи» — я инженер механик + неплохой слесарь с 20-летним стажем. Сварку осваивал сам, поскольку люблю строить различные вещи (мото, авто и др.). Но только с появлением современного сварочного оборудования мои работы смогли шагнуть на более высокий уровень. Надо отдать должное — этому я обязан своему куму. Именно с его подачи в мастерской появился комбинированный сварочный аппарат и маска «хамелеон». Но вернемся к нашим баранам... ой, простите, драконам.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-33323600-1390764009.jpg" data-fileid="28102" data-fileext="jpg" rel=""><img data-fileid="28102" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-33323600-1390764009_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-33323600-1390764009_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-29115800-1390764043.jpg" data-fileid="28103" data-fileext="jpg" rel=""><img data-fileid="28103" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-29115800-1390764043_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-29115800-1390764043_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-80479000-1390765633.jpg" data-fileid="28116" data-fileext="jpg" rel=""><img data-fileid="28116" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-80479000-1390765633_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-80479000-1390765633_thumb.jpg"></a></p><p> </p><p>
Давно хотел сделать что-то типа чужого или хищника, но поскольку эта тема уже жевана-пережевана, решил свое. Так вот одел я значит наряд волшебника (маска, перчатки), взял волшебную палочку (горелка полуавтомата) и понеслась.</p><p> </p><p>
<strong>Первый дракон МОТОЦЕРАПТОР (прототип велоцераптор).</strong></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-05843600-1390763939.jpg" data-fileid="28100" data-fileext="jpg" rel=""><img data-fileid="28100" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-05843600-1390763939_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-05843600-1390763939_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-78706600-1390763972.jpg" data-fileid="28101" data-fileext="jpg" rel=""><img data-fileid="28101" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-78706600-1390763972_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-78706600-1390763972_thumb.jpg"></a></p><p> </p><p>
Так в процессе археологических изысканий, в подвалах и катакомбах моей базы, были обнаружены фрагменты грозного хищника МОТОЦЕРАПТОРА. При помощи полуавтомата и шлифмашинки проведено генно-сварочное реконструирование и оживление зверя. Голова — дырявый бак от «вайпер актив» (есть такой гаражный заводик на густозаселенных просторах Китая — клепают тама мопеды относительной прочности). Зубы — свечи зажигания, глаза — обоймы и шарики с подшипников качения. Тело динозавра — два бака от скутеров (как и на драконе так и в жизни ЯМАХА и ХОНДА они составляют костяк — ну прочные дюже), спина — это дно от бака «хонды ДИО», а пузо — бак от старой «ямашки». Шея — основа труба от старого смывного бачка (ну как обойтись без легенды Русского тюнинга). Ну а сверху нанизаны цилиндры от 200-ки мотокитаезы, 125-ки, ну и 72 кубика (скутерные). Теперь ноги — точнее-НОГЫ — с такими когтями последнее правильнее. Когти плавно переходящие в пальцы — это порезанные коуши для строповки. Бедра нашего красавца — это глушитель с китайского скутера. Я бы назвал его мечтой сварщика (больно тонкий, да и металл пахабный). Колени — чашки сцепления скутеров, голени — остатки трубы с толчка. Руки — шатуны с еще одной легенды СОЮЗсамопалтюнинг — ЗАПОРОЖЦА (накануне ставил одному ученому изобретателю на запор новейший электродвигатель, вот шатуны и валялись в мастерской). Ну а теперь как в мультике: РУКИ, НОГИ?! — ГЛАВНОЕ ХВОСТ! Хвост — каркас из полос, а сверху цепи с мотоциклов. Для придания жесткости (баки все же с жести и гнет их в околошовной зоне, шея особенно) по хребту пустил звездочки с мото. Ну а сверху украсил цепями от бензопил и цепями ГРМ от скутеров (ну не может быть динозавр гладким и не гадким-колючим).</p><p> </p><p>
И так господа, поехали дальше: <strong>ЯПОНСКИЙ ДРАКОН</strong>!</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-62136600-1390765153.jpg" data-fileid="28104" data-fileext="jpg" rel=""><img data-fileid="28104" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-62136600-1390765153_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-62136600-1390765153_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-46488300-1390765179.jpg" data-fileid="28105" data-fileext="jpg" rel=""><img data-fileid="28105" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-46488300-1390765179_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-46488300-1390765179_thumb.jpg"></a></p><p> </p><p>
С момента постройки Эйфелевой башни в моей голове сидела мысль сделать толи змею, толи дракона из одних цепей. И вот, наконец, мои тараканы в голове мутировали в дракончиков и наслали на меня вдохновения. Результат на фото: 80 метров цепей, более 5000 точек сварки и первый в мире дракон из цепей — японский дракон родился на свет. Для тех, кто захочет работать с цепями, совет: цепи старые с износом позволяют их крутить и гнуть, а перед работой я их отжигаю в буржуйке (смазка выгорает и ржавчина тоже, да и цепи отпускаются). Только потом цепь надо отбить об наковальню от шлака (не забываем об том, даже на нашем САЙТЕ запасных глаз не продают — очки лучше одеть). Схему постройки видно из фоток. На листе металла нарисовал силуэт тела дракона, по нему сварил каркас из проволоки (очень важно: стол из металла — цепи садят напругу, или двигайте зажим массы). И потом варим, варим, варим — одну половинку. По ходу отбрехиваемся от банды «хомячков» умников. Кстати ХОМЯЧОК — тело трындящее под руку. Высший разряд ХОМЯЧОК ГАРАЖНЫЙ — стебно-трындящий со знанием дела. После полной сборки половинки оную переворачиваем, провариваем поперек цепей с шагом в 100 мм. Затем привариваем к готовой половинке каркас, срезанный с листа, и поехали далее (для удобства я все цепи разложил на полу, так виднее; отдельно сильно изношенные с большим люфтом цепи — их на гибах крутить удобнее).</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-27719000-1390765517.jpg" data-fileid="28111" data-fileext="jpg" rel=""><img data-fileid="28111" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-27719000-1390765517_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-27719000-1390765517_thumb.jpg"></a></p><p> </p><p>
Момент, когда тело было собрано и лежало на боку — это самый пошло-эротичный период. Каждый примерял, при этом перечислял все хитрые жопы достойные этого инструмента. Пришлось срочно вывешивать над столом и колдовать ноги.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-65861100-1390765540.jpg" data-fileid="28113" data-fileext="jpg" rel=""><img data-fileid="28113" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-65861100-1390765540_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-65861100-1390765540_thumb.jpg"></a></p><p> </p><p>
Пальцы — это шатуны от москвича, а большие пальцы от «21 волги». Основа ног — 38-я труба. Для равномерной текстуры пришлось проходить в два слоя цепями: низ мото, а наружный слой велосипедными цепями.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-50359200-1390765528.jpg" data-fileid="28112" data-fileext="jpg" rel=""><img data-fileid="28112" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-50359200-1390765528_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-50359200-1390765528_thumb.jpg"></a></p><p> </p><p>
Над головой дракона пришлось поломать и почесать свою балбешку. Решил начать с челюстей, сделал одну, по ней чуть больше верхнюю. Клыки — шатуны с скутеров «Сузуки». Передние резцы — цепь столярного фрезера, остальное — цепи бензопил. Ноздри — пальцы с поршней двигателя БМВ, глаза — шаровые пальцы с иномарки (модель AHEZ — А Хрен Его Знает — главное на донышке зрачки готовые). На гребни и бороду пошли велосипедные звездочки.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-24575400-1390765472.jpg" data-fileid="28108" data-fileext="jpg" rel=""><img data-fileid="28108" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-24575400-1390765472_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-24575400-1390765472_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-49349900-1390765486.jpg" data-fileid="28109" data-fileext="jpg" rel=""><img data-fileid="28109" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-49349900-1390765486_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-49349900-1390765486_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-70594500-1390765502.jpg" data-fileid="28110" data-fileext="jpg" rel=""><img data-fileid="28110" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-70594500-1390765502_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-70594500-1390765502_thumb.jpg"></a></p><p> </p><p>
Краска хаммерит, грунт ГФ. Скажу сразу: такую работу стоит затевать только при наличии маски хамелеона и хорошего полуавтомата. Отдельно напомню: АККУРАТНО люди при резке цепей! Крепим в тиса, а не режем навесу.</p><p> </p><p>
<strong>ЗМЕЙ ГОРЫНЫЧ!</strong></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-04316700-1390833268.jpg" data-fileid="28154" data-fileext="jpg" rel=""><img data-fileid="28154" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-04316700-1390833268_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-04316700-1390833268_thumb.jpg"></a></p><p> </p><p>
Да, это не самая сложная из моих работ, но наиболее позитивная и самая моя любимая. Чем примечателен Горыныч — это не просто сказка, это детство... детство каждого из нас. Ведь головы — это баки от мопедов: Карпаты, Верховина (на средней голове специально оставил таблички). И кто не улыбнется, вспоминая, как в детстве колупал эти пропахшие бензином и маслом двухколесные ракеты, а потом толкал с друзьями на школьном дворе. А брюхо — бак от К750. Как круто было в деревне укатить у деда «тяж» за угол и сгонять на ставок покупаться ночью (очень пришлось в пору при работе то, что он самый толстостенный). Медальон на груди — дань рекламе кореша стоматолога. Спина — это целая эпопея. ИЖжога — бак с ижака, на котором с друзьями мотались на рыбалку, а бензина мало, долили соляры — результат дымит, а не едет и толкай его на бугор. Для визуального соединения двух баков опоясал цепью-ремнем. Хвост — это более 20 метров цепей. Здесь попробовал работать без каркаса — сначала вроде ничего, а вот в конце тяжело сводить плавно верх и низ. Гребни — из велосипедных звездочек (для безопасности накрыл поверху цепью). Крылья вырезал из листа — по периметру трубка и пруток. Все три шеи — это цилиндры со скутеров, нанизанные на 38 трубу. На все три головы 128 зубов — это свечи зажигания (авто, мото, бензопилы). Руки — это рычаги подвески с трактора, для антуража на палец я сделал кольцо. На пряжке ремня инициалы вашего покорного слуги. Ноги: бедра-глушители великокитайских скутеров, голени — мазовские шатуны, пальцы — шатуны а/м москвич.</p><p> </p><p>
На покраску привлек сына — пусть учится, да и стоит Горыныч недалеко от школы — не стыдно Димке перед одноклассниками — тоже руку приложил.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-79977400-1390765593.jpg" data-fileid="28114" data-fileext="jpg" rel=""><img data-fileid="28114" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-79977400-1390765593_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-79977400-1390765593_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-34170500-1390765610.jpg" data-fileid="28115" data-fileext="jpg" rel=""><img data-fileid="28115" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-34170500-1390765610_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-34170500-1390765610_thumb.jpg"></a></p><p> </p><p>
Скажу так: главное в этой работе — это радость, которую Горыныч дарит людям. И он вам УЛЫБАЕТСЯ — он свой корешь! Свой в доску!</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-54133500-1390765662.jpg" data-fileid="28117" data-fileext="jpg" rel=""><img data-fileid="28117" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-54133500-1390765662_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-54133500-1390765662_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-15550500-1390765692.jpg" data-fileid="28118" data-fileext="jpg" rel=""><img data-fileid="28118" class="ipsImage ipsImage_thumbnailed" alt="post-8109-0-15550500-1390765692_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-8109-0-15550500-1390765692_thumb.jpg"></a></p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа № 18</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p> </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p> </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p> </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3734</guid><pubDate>Mon, 27 Jan 2014 14:28:07 +0000</pubDate></item><item><title>&#x411;&#x440;&#x430;&#x442;&#x44C;&#x44F; &#x421;&#x442;&#x430;&#x43B;&#x438;</title><link>https://websvarka.ru/talk/topic/3727-bratya-stali/</link><description><![CDATA[
<p>На форуме я новичек, пришел сюда почитать по сварке труб малого диаметра - для дома, для семьи. Утилитарные вещи делаю по необходимости, но иногда чего-то ваяю для души. К примеру, вот:</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11140-0-62221500-1390645391.jpg" data-fileid="27916" data-fileext="jpg" rel=""><img data-fileid="27916" class="ipsImage ipsImage_thumbnailed" alt="post-11140-0-62221500-1390645391_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11140-0-62221500-1390645391_thumb.jpg"></a></p><p> </p><p>
Сделаны фигурки из обносков железа. Если приглядеться, его качество видно. Но не облезли, так как купались в преобразователе ржавчины. Фигурки каркасные из оббитых стержней электродов УОНИ13/55 производства ЛЭЗ. Для сварки ими у меня не хватает навыка, как высказался один сварщик, они для адекватного оборудования (имея ввиду под ним многопостовик на 1600А). Но у меня его нету, а выкидывать жалко, вот и пошли в дело. Уони других производителей применялись и в этой конструкции так как ноги и часть торса — арматура 12 мм. Все остальное тоже РДС электродами всеми, что лежали в колчане и ОМНИА46 крылья, и АНО4 точки крепления перьев, и АНО21 подводка глаз и носа.</p><p>
 </p><p>
Пернатых делал несколько разных, они не по шаблону, а с руки. Есть несколько фоток при плохом освещении в месте изготовления </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11140-0-51728000-1390645568.jpg" data-fileid="27917" data-fileext="jpg" rel=""><img data-fileid="27917" class="ipsImage ipsImage_thumbnailed" alt="post-11140-0-51728000-1390645568_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11140-0-51728000-1390645568_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11140-0-91755600-1390645570.jpg" data-fileid="27918" data-fileext="jpg" rel=""><img data-fileid="27918" class="ipsImage ipsImage_thumbnailed" alt="post-11140-0-91755600-1390645570_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11140-0-91755600-1390645570_thumb.jpg"></a> </p><p>
 </p><p>
Моська крупным планом, это филиня <img alt=":)" src="https://websvarka.ru/talk/uploads/emoticons/default_smile.png"></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11140-0-10102700-1390645573.jpg" data-fileid="27919" data-fileext="jpg" rel=""><img data-fileid="27919" class="ipsImage ipsImage_thumbnailed" alt="post-11140-0-10102700-1390645573_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11140-0-10102700-1390645573_thumb.jpg"></a></p><p> </p><p>
Прежде чем наводить марафет, нужно помыться</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-33870600-1390728476.jpg" data-fileid="28035" data-fileext="jpg" rel=""><img data-fileid="28035" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-33870600-1390728476_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-33870600-1390728476_thumb.jpg"></a></p><p> </p><p>
Теперича можно принять должную окраску:-)</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-48779300-1390728571.jpg" data-fileid="28037" data-fileext="jpg" rel=""><img data-fileid="28037" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-48779300-1390728571_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-48779300-1390728571_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-48890600-1390728570.jpg" data-fileid="28036" data-fileext="jpg" rel=""><img data-fileid="28036" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-48890600-1390728570_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-48890600-1390728570_thumb.jpg"></a></p><p> </p><p>
И на пост</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-04076400-1390728667.jpg" data-fileid="28038" data-fileext="jpg" rel=""><img data-fileid="28038" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-04076400-1390728667_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-04076400-1390728667_thumb.jpg"></a></p><p>
 </p><p>
Фото по отдельности. На посту спустя 1.5 года после установки</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11140-0-46142700-1390645284.jpg" data-fileid="27914" data-fileext="jpg" rel=""><img data-fileid="27914" class="ipsImage ipsImage_thumbnailed" alt="post-11140-0-46142700-1390645284_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11140-0-46142700-1390645284_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11140-0-52335900-1390645287.jpg" data-fileid="27915" data-fileext="jpg" rel=""><img data-fileid="27915" class="ipsImage ipsImage_thumbnailed" alt="post-11140-0-52335900-1390645287_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11140-0-52335900-1390645287_thumb.jpg"></a></p><p> </p><p>
Есть и еще мысли, но свободного металлолома нету. Эти мейд ин сварка болгарка да обрезки были. Ну примерно так.</p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа №16</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3727</guid><pubDate>Sun, 26 Jan 2014 13:56:25 +0000</pubDate></item><item><title>&#x421;&#x430;&#x43C;&#x43E;&#x434;&#x435;&#x43B;&#x44C;&#x43D;&#x44B;&#x439; &#x43E;&#x442;&#x432;&#x430;&#x43B;</title><link>https://websvarka.ru/talk/topic/3868-samodelnyy-otval/</link><description><![CDATA[
<p>Так-как одним из критериев конкурса является то, что изделие должно быть полезным и функциональным, я решил показать отвал.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-79251900-1392022727.jpg" data-fileid="29735" data-fileext="jpg" rel=""><img data-fileid="29735" class="ipsImage ipsImage_thumbnailed" alt="post-1894-0-79251900-1392022727_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-79251900-1392022727_thumb.jpg"></a></p><p> </p><p>
Снег выпадать не хочет, видео пока не будет и человек не захотел просто так, выгонять грузовичок, надо прогревать и т.д. Немного предыстории.</p><p>
Изначально, заказчик вместе с батей, сами забацали отвал, но у них согнуло крепление. Крепление я сделал новое прошлой осенью. Не выдержал сам отвал, на новом крепление. Этой осенью я сделал новый отвал, который был уже испробован и показал себя нормально.</p><p> </p><p>
Крепление было сделано и подогнано примерно за 4-5 часов, на отвал ушло примерно столько же времени, ну и ещё пару часов на доделку-придумку крепления пружин и мелочи. Отвал поворачивается влево-право и вверх-низ. Это было сделано, чтобы не погнуло раму при серьёзном препятствии. Отвал загибается вниз, почти параллельно земле, назад его оттягивают пружины.</p><p> </p><p>
Материалы: лист тройки, размер был 2000х600мм, размер отвала — 2000х500мм. Было сделано 4 надреза и загнуто на бордюре (для питерских — на пареблике))) с помощью кувалды, потом проварено. Трубопрофиль 60х40х3 мм.  60х30х3мм; 40х25х2мм. </p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-22238000-1392022354.jpg" data-fileid="29726" data-fileext="jpg" rel=""><img data-fileid="29726" class="ipsImage ipsImage_thumbnailed" alt="post-1894-0-22238000-1392022354_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-22238000-1392022354_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-03229300-1392022375.jpg" data-fileid="29727" data-fileext="jpg" rel=""><img data-fileid="29727" class="ipsImage ipsImage_thumbnailed" alt="post-1894-0-03229300-1392022375_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-03229300-1392022375_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-64482200-1392022402.jpg" data-fileid="29728" data-fileext="jpg" rel=""><img data-fileid="29728" class="ipsImage ipsImage_thumbnailed" alt="post-1894-0-64482200-1392022402_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-64482200-1392022402_thumb.jpg"></a> <a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-40206800-1392022422.jpg" data-fileid="29729" data-fileext="jpg" rel=""><img data-fileid="29729" class="ipsImage ipsImage_thumbnailed" alt="post-1894-0-40206800-1392022422_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-40206800-1392022422_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-96908800-1392022441.jpg" data-fileid="29730" data-fileext="jpg" rel=""><img data-fileid="29730" class="ipsImage ipsImage_thumbnailed" alt="post-1894-0-96908800-1392022441_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-96908800-1392022441_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-61017400-1392022509.jpg" data-fileid="29731" data-fileext="jpg" rel=""><img data-fileid="29731" class="ipsImage ipsImage_thumbnailed" alt="post-1894-0-61017400-1392022509_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-61017400-1392022509_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-38983400-1392022565.jpg" data-fileid="29732" data-fileext="jpg" rel=""><img data-fileid="29732" class="ipsImage ipsImage_thumbnailed" alt="post-1894-0-38983400-1392022565_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-38983400-1392022565_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-04888600-1392022627.jpg" data-fileid="29733" data-fileext="jpg" rel=""><img data-fileid="29733" class="ipsImage ipsImage_thumbnailed" alt="post-1894-0-04888600-1392022627_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-04888600-1392022627_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-59611800-1392022691.jpg" data-fileid="29734" data-fileext="jpg" rel=""><img data-fileid="29734" class="ipsImage ipsImage_thumbnailed" alt="post-1894-0-59611800-1392022691_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-59611800-1392022691_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-05435500-1392022776.jpg" data-fileid="29736" data-fileext="jpg" rel=""><img data-fileid="29736" class="ipsImage ipsImage_thumbnailed" alt="post-1894-0-05435500-1392022776_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-05435500-1392022776_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-38538500-1392022808.jpg" data-fileid="29737" data-fileext="jpg" rel=""><img data-fileid="29737" class="ipsImage ipsImage_thumbnailed" alt="post-1894-0-38538500-1392022808_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_02_2014/post-1894-0-38538500-1392022808_thumb.jpg"></a></p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа № 49</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3868</guid><pubDate>Wed, 12 Feb 2014 17:06:43 +0000</pubDate></item><item><title>&#x41F;&#x43E;&#x434;&#x430;&#x440;&#x43E;&#x447;&#x43D;&#x430;&#x44F; &#x440;&#x43E;&#x437;&#x430;</title><link>https://websvarka.ru/talk/topic/3674-podarochnaya-roza/</link><description><![CDATA[
<p>Всем доброго времени суток! Меня зовут Сергей, я студент-инженер, 21 год. Хочу представить мою работу на Ваш суд.</p><p>
 </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11078-0-22907200-1390163015.jpg" data-fileid="27579" data-fileext="jpg" rel=""><img data-fileid="27579" class="ipsImage ipsImage_thumbnailed" alt="post-11078-0-22907200-1390163015_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11078-0-22907200-1390163015_thumb.jpg"></a></p><p>
 </p><p>
На сайте я совсем недавно, так как пришлось обращаться за помощью по вопросам отопления. А тут конкурс... Сделана роза не специально для конкурса, а в подарок моей девушке. Подарок, мягко говоря, понравился.</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11078-0-34872100-1390161452.jpg" data-fileid="27578" data-fileext="jpg" rel=""><img data-fileid="27578" class="ipsImage ipsImage_thumbnailed" alt="post-11078-0-34872100-1390161452_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11078-0-34872100-1390161452_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11078-0-80934700-1390163047.jpg" data-fileid="27580" data-fileext="jpg" rel=""><img data-fileid="27580" class="ipsImage ipsImage_thumbnailed" alt="post-11078-0-80934700-1390163047_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11078-0-80934700-1390163047_thumb.jpg"></a></p><p>
 </p><p>
Изготовлена из листового металла старого, но рабочего холодильника. Теперь он выглядит как то так:</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11078-0-79356800-1390163144.jpg" data-fileid="27581" data-fileext="jpg" rel=""><img data-fileid="27581" class="ipsImage ipsImage_thumbnailed" alt="post-11078-0-79356800-1390163144_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11078-0-79356800-1390163144_thumb.jpg"></a></p><p>
 </p><p>
Варил порядка 12-ти часов в течение 3-х дней. Путь от холодильника до подарка остался лишь у меня в голове (фотографий изготовления не осталось). Холодильник рабочий — сам замерял температуру, -20 градусов мороза показывает <img alt=":pleasantry:" src="https://websvarka.ru/talk/uploads/emoticons/default_pleasantry.gif"></p><p>
 </p><p>
Еще не крашеная в моей руке</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11078-0-73895900-1390163392.jpg" data-fileid="27582" data-fileext="jpg" rel=""><img data-fileid="27582" class="ipsImage ipsImage_thumbnailed" alt="post-11078-0-73895900-1390163392_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11078-0-73895900-1390163392_thumb.jpg"></a> </p><p>
 </p><p>
Смотрите, любуйтесь, оставляйте комментарии, можно немножко покритиковать.</p><p>
 </p><p>
Занимаюсь подобными вещами не так давно. Варю ручной дуговой. Кину еще пару фото из моих работ этого направления:</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11078-0-30641700-1390163958.jpg" data-fileid="27583" data-fileext="jpg" rel=""><img data-fileid="27583" class="ipsImage ipsImage_thumbnailed" alt="post-11078-0-30641700-1390163958_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11078-0-30641700-1390163958_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11078-0-29202200-1390164075.jpg" data-fileid="27584" data-fileext="jpg" rel=""><img data-fileid="27584" class="ipsImage ipsImage_thumbnailed" alt="post-11078-0-29202200-1390164075_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-11078-0-29202200-1390164075_thumb.jpg"></a></p><p>
 </p><p>
</p><hr><p>
<strong>Конкурсная работа №9</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3674</guid><pubDate>Mon, 20 Jan 2014 10:14:13 +0000</pubDate></item><item><title>&#x41A;&#x430;&#x440;&#x435;&#x442;&#x430; &#x43B;&#x438;&#x43C;&#x443;&#x437;&#x438;&#x43D;</title><link>https://websvarka.ru/talk/topic/3654-kareta-limuzin/</link><description><![CDATA[
<p>Здравствуйте Уважаемые форумчане и Жюри  моего проекта!</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-08889100-1389979517.jpg" data-fileid="27366" data-fileext="jpg" rel=""><img data-fileid="27366" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-08889100-1389979517_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-08889100-1389979517_thumb.jpg"></a></p><p> </p><p>
Меня зовут Дмитрий. Я из Челябинска. Женат, жду со дня на день прибавление в семье. Строю своими руками дом для своей семьи и для этого решил поучаствовать в конкурсе. Я творческий человек и хочу рассказать о своем детище которое создал сам своими руками (от эскиза до воплощения в реале) под названием: Карета лимузин.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-01332900-1389979519.jpg" data-fileid="27369" data-fileext="jpg" rel=""><img data-fileid="27369" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-01332900-1389979519_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-01332900-1389979519_thumb.jpg"></a></p><p> </p><p>
Это мой первый проект который я предоставляю на публику. Возможно, это даст толчок кому-то для развития новых изобретений из автомобилей, которые можно создать своими руками и воплотить их в жизнь. Я рад что выбрал свою профессию Сварщика! Я очень горд этим, горд тем, что я сам своими руками создаю то, что  завтра будет радовать людей и на моей будущей карете наверняка будут делать первое признание в Любви, играть свадьбы, забирать детей с роддома!  </p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-23546400-1389979516.jpg" data-fileid="27364" data-fileext="jpg" rel=""><img data-fileid="27364" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-23546400-1389979516_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-23546400-1389979516_thumb.jpg"></a></p><p> </p><p>
Весь проект занял несколько месяцев: от эскиза до воплощение мечты. Первоначально автомобиль крайслер 300 был разрезан пополам. После создано днище автомобиля. Был  создан шаблон для проекции каркаса кареты, создан сам каркас. Установлен каркас на автомобиль. На протяжении нескольких месяцев зашит каркас.</p><p>
 </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-01826600-1389979518.jpg" data-fileid="27367" data-fileext="jpg" rel=""><img data-fileid="27367" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-01826600-1389979518_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-01826600-1389979518_thumb.jpg"></a> <a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-95599500-1389979514.jpg" data-fileid="27362" data-fileext="jpg" rel=""><img data-fileid="27362" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-95599500-1389979514_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-95599500-1389979514_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-57628900-1389979515.jpg" data-fileid="27363" data-fileext="jpg" rel=""><img data-fileid="27363" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-57628900-1389979515_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-57628900-1389979515_thumb.jpg"></a></p><p> </p><p>
А это видео кареты</p><p>
<a href="http://www.youtube.com/watch?v=eJhXTjEpHuo" rel="external nofollow">http://www.youtube.com/watch?v=eJhXTjEpHuo</a></p><p> </p><p>
Помимо этого хочу выложить несколько фото моих предыдущих работ которые я создал своими руками.  </p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-54222300-1389979518.jpg" data-fileid="27368" data-fileext="jpg" rel=""><img data-fileid="27368" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-54222300-1389979518_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-54222300-1389979518_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-68288400-1389979516.jpg" data-fileid="27365" data-fileext="jpg" rel=""><img data-fileid="27365" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-68288400-1389979516_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-68288400-1389979516_thumb.jpg"></a></p><p> </p><p>
Уважаемые друзья, коллеги и  жюри! Надеюсь, вы оцените мою работу и отдадите свой голос за меня!</p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа №4</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3654</guid><pubDate>Fri, 17 Jan 2014 16:36:48 +0000</pubDate></item><item><title>&#x414;&#x438;&#x43D;&#x43E;&#x437;&#x430;&#x432;&#x440;</title><link>https://websvarka.ru/talk/topic/3725-dinozavr/</link><description><![CDATA[
<p>Добрый день всем. Долго думал и решил выполнить работу специально для конкурса Вебсварки «Сделано своими руками».</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-32668900-1390663908.jpg" data-fileid="27957" data-fileext="jpg" rel=""><img data-fileid="27957" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-32668900-1390663908_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-32668900-1390663908_thumb.jpg"></a></p><p> </p><p>
Перебирал несколько видов материалов: черная сталь, алюминий, нержавейка, титан, но это вроде как каждодневно обиходные материалы. И тут в гараже нашел кусок листа медного мр-3 толщиной 0,8 мм. Когда-то отец им колонку газовую переклепывал, лет тридцать валялся, ну и решил я его оживить. Вся работа сделана из листа аргонодуговой сваркой. Изготовление заняло где-то неделю времени. Думаю, в этой роботе зацепил все: сварку, слесарку, художество и даже полезность. Получилась хорошая игрушка, дети в очереди стоят кому достанется. В общем вот такой динозавр получился.</p><p> </p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-17529700-1390663930.jpg" data-fileid="27958" data-fileext="jpg" rel=""><img data-fileid="27958" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-17529700-1390663930_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-17529700-1390663930_thumb.jpg"></a></p><p> </p><p>
Пару фото с разных сторон:</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-44013600-1390663963.jpg" data-fileid="27964" data-fileext="jpg" rel=""><img data-fileid="27964" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-44013600-1390663963_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-44013600-1390663963_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-05596100-1390663963.jpg" data-fileid="27963" data-fileext="jpg" rel=""><img data-fileid="27963" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-05596100-1390663963_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-05596100-1390663963_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-64982900-1390663962.jpg" data-fileid="27962" data-fileext="jpg" rel=""><img data-fileid="27962" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-64982900-1390663962_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-64982900-1390663962_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-22001500-1390663962.jpg" data-fileid="27961" data-fileext="jpg" rel=""><img data-fileid="27961" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-22001500-1390663962_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-22001500-1390663962_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-71423500-1390663961.jpg" data-fileid="27960" data-fileext="jpg" rel=""><img data-fileid="27960" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-71423500-1390663961_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-71423500-1390663961_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-77316800-1390663960.jpg" data-fileid="27959" data-fileext="jpg" rel=""><img data-fileid="27959" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-77316800-1390663960_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-77316800-1390663960_thumb.jpg"></a></p><p> </p><p>
Но, как мне кажется, сам процесс изготовления намного интересней самого изделия.</p><p> </p><p>
Так все начиналось — из инструментов ножницы и пару мультитулов</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-71543800-1390664078.jpg" data-fileid="27966" data-fileext="jpg" rel=""><img data-fileid="27966" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-71543800-1390664078_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-71543800-1390664078_thumb.jpg"></a></p><p> </p><p>
Первая нога выгнута</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-18377300-1390664079.jpg" data-fileid="27967" data-fileext="jpg" rel=""><img data-fileid="27967" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-18377300-1390664079_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-18377300-1390664079_thumb.jpg"></a></p><p> </p><p>
За первый день нагнул почти все заготовки</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-24948300-1390664078.jpg" data-fileid="27965" data-fileext="jpg" rel=""><img data-fileid="27965" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-24948300-1390664078_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-24948300-1390664078_thumb.jpg"></a></p><p> </p><p>
День второй — наобдирал проводов (на присадку 2мм) и приступил к сварке</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-64247700-1390664079.jpg" data-fileid="27968" data-fileext="jpg" rel=""><img data-fileid="27968" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-64247700-1390664079_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-64247700-1390664079_thumb.jpg"></a></p><p> </p><p>
Первые детали после сборки-прихватки</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-91665200-1390664153.jpg" data-fileid="27969" data-fileext="jpg" rel=""><img data-fileid="27969" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-91665200-1390664153_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-91665200-1390664153_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-39384100-1390664154.jpg" data-fileid="27970" data-fileext="jpg" rel=""><img data-fileid="27970" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-39384100-1390664154_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-39384100-1390664154_thumb.jpg"></a></p><p> </p><p>
Внутри пустота</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-96660800-1390664179.jpg" data-fileid="27971" data-fileext="jpg" rel=""><img data-fileid="27971" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-96660800-1390664179_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-96660800-1390664179_thumb.jpg"></a></p><p> </p><p>
Результат первого дня</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-20135900-1390664200.jpg" data-fileid="27972" data-fileext="jpg" rel=""><img data-fileid="27972" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-20135900-1390664200_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-20135900-1390664200_thumb.jpg"></a></p><p> </p><p>
Зачистка, рихтовка, подгонка</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-87916700-1390664239.jpg" data-fileid="27973" data-fileext="jpg" rel=""><img data-fileid="27973" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-87916700-1390664239_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-87916700-1390664239_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-31795400-1390664240.jpg" data-fileid="27974" data-fileext="jpg" rel=""><img data-fileid="27974" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-31795400-1390664240_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-31795400-1390664240_thumb.jpg"></a></p><p> </p><p>
Соединение «больших» узлов - ноги, хвост, туловище</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-67173700-1390664265.jpg" data-fileid="27975" data-fileext="jpg" rel=""><img data-fileid="27975" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-67173700-1390664265_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-67173700-1390664265_thumb.jpg"></a></p><p> </p><p>
Ближе к окончанию. Все собрано в кучу, дальше сварка</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-18700200-1390664322.jpg" data-fileid="27976" data-fileext="jpg" rel=""><img data-fileid="27976" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-18700200-1390664322_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-18700200-1390664322_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-81712500-1390664328.jpg" data-fileid="27977" data-fileext="jpg" rel=""><img data-fileid="27977" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-81712500-1390664328_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-81712500-1390664328_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-71022100-1390664338.jpg" data-fileid="27978" data-fileext="jpg" rel=""><img data-fileid="27978" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-71022100-1390664338_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-71022100-1390664338_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-85102300-1390664340.jpg" data-fileid="27979" data-fileext="jpg" rel=""><img data-fileid="27979" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-85102300-1390664340_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-85102300-1390664340_thumb.jpg"></a></p><p> </p><p>
Это случайная жертва - для размера</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-47367600-1390664385.jpg" data-fileid="27981" data-fileext="jpg" rel=""><img data-fileid="27981" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-47367600-1390664385_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-47367600-1390664385_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-72926100-1390664384.jpg" data-fileid="27980" data-fileext="jpg" rel=""><img data-fileid="27980" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-72926100-1390664384_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-72926100-1390664384_thumb.jpg"></a></p><p> </p><p>
Полная обварка</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-87080700-1390664438.jpg" data-fileid="27982" data-fileext="jpg" rel=""><img data-fileid="27982" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-87080700-1390664438_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-87080700-1390664438_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-26912500-1390664439.jpg" data-fileid="27983" data-fileext="jpg" rel=""><img data-fileid="27983" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-26912500-1390664439_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-26912500-1390664439_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-69278600-1390664439.jpg" data-fileid="27984" data-fileext="jpg" rel=""><img data-fileid="27984" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-69278600-1390664439_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-69278600-1390664439_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-11291800-1390664440.jpg" data-fileid="27985" data-fileext="jpg" rel=""><img data-fileid="27985" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-11291800-1390664440_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-11291800-1390664440_thumb.jpg"></a></p><p> </p><p>
Окончательная зачистка и шлифовка</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-63264100-1390664492.jpg" data-fileid="27986" data-fileext="jpg" rel=""><img data-fileid="27986" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-63264100-1390664492_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-63264100-1390664492_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-06564400-1390664493.jpg" data-fileid="27987" data-fileext="jpg" rel=""><img data-fileid="27987" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-06564400-1390664493_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-06564400-1390664493_thumb.jpg"></a></p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-46284900-1390664493.jpg" data-fileid="27988" data-fileext="jpg" rel=""><img data-fileid="27988" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-46284900-1390664493_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-46284900-1390664493_thumb.jpg"></a><a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-86260500-1390664493.jpg" data-fileid="27989" data-fileext="jpg" rel=""><img data-fileid="27989" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-86260500-1390664493_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-86260500-1390664493_thumb.jpg"></a></p><p> </p><p>
Лень было ехать еще раз греть сваркой, затемняю на плите</p><p>
<a class="ipsAttachLink ipsAttachLink_image" href="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-49468300-1390664517.jpg" data-fileid="27990" data-fileext="jpg" rel=""><img data-fileid="27990" class="ipsImage ipsImage_thumbnailed" alt="post-1-0-49468300-1390664517_thumb.jpg" src="https://websvarka.ru/talk/uploads/monthly_01_2014/post-1-0-49468300-1390664517_thumb.jpg"></a></p><p> </p><p>
Надеюсь, кому-нибудь понравится. А в общем благодаря этому конкурсу заставил себя оторвать зад от стула и сделать что-нибудь этакое... давно хотел - так что для себя я уже победил.</p><p> </p><p>
Видео: на улице -12-15... Динозавр был рожден в экстрим условиях.</p><p>
<a href="https://www.youtube.com/watch?v=E-Wp-7j8d1Q" rel="external nofollow">https://www.youtube.com/watch?v=E-Wp-7j8d1Q</a></p><p> </p><p>
</p><hr><p>
<strong>Конкурсная работа №14</strong>, предоставлена в рамках <a href="http://websvarka.ru/talk/index.php?showtopic=3626" rel="external nofollow">Конкурса «Сделано своими руками»</a></p><p>
 </p><p>
<strong>Спонсоры Конкурса</strong></p><p>
<a href="http://resanta.ru/" rel="external nofollow">Ресанта</a> — ведущий поставщик электрооборудования для сварки, тепла и комфорта.</p><p>
<a href="http://resanta.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_resanta_300.jpg</span></a></p><p>
 </p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow">Тиберис</a> — первый интернет-гипермаркет сварочного оборудования.</p><p>
<a href="http://www.tiberis.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_tiberis_200.jpg</span></a></p><p>
 </p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow">Евротек</a> — интернет-магазин строительного оборудования.</p><p>
<a href="http://evrotek.spb.ru/" rel="external nofollow"><span>http://websvarka.ru/images/forum/konkurs_evrotek_130.jpg</span></a></p>
]]></description><guid isPermaLink="false">3725</guid><pubDate>Sat, 25 Jan 2014 15:45:52 +0000</pubDate></item></channel></rss>